Preparation method of thermal-oxidation-resistant and impact-resistant polyamide hot melt adhesive

By combining modified polyamide with copper diethylphosphinate and other materials, a heat-resistant oxidation-resistant polyamide hot melt adhesive was prepared, which solved the problems of degradation of mechanical properties and thermal oxidation degradation of polyamide hot melt adhesives, which significantly Improves its impact and heat resistance.

CN118931472AInactive Publication Date: 2024-11-12TIANJIN FUXIN CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197924.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyamide hot melt adhesives are prone to deterioration of mechanical properties and thermal oxidation degradation during storage, transportation and use. They are low in toughness and strong hydrophilicity, making them difficult to meet the needs of thermal oxidation and impact resistance.

Method used

The molecular chain of modified polyamide is prepared by melt copolycondensation method by combining modified polyamide with cuprous diethylphosphonite, epoxy resin and zinc stearate. More flexible, the redox cycle of Cu+ ions inhibits free radicals and enhances the thermal oxidation and impact resistance of the polymer.

Benefits of technology

It improves the impact resistance and mechanical properties of polyamide hot melt adhesive, reduces the thermal oxidation and degradation rate, enhances its stability in thermal and oxygen environments, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017026970000061
    Figure BDA0005017026970000061
Patent Text Reader

Abstract

The invention relates to a preparation method of a thermal-oxidation-resistant and impact-resistant polyamide hot melt adhesive, and belongs to the technical field of hot melt adhesives, and the hot melt adhesive is prepared from polyamide, modified polyamide, cuprous diethyl phosphonite, epoxy resin and zinc stearate. Wherein the modified polyamide is prepared by polymerizing CPL, PA1012 salt and deionized water, and the PA1012 salt is prepared by mixing an ethanol solution of 1, 10-decane dicarboxylic acid and an ethanol solution of 1, 10-diaminodecane. Under the conditions of heat and oxygen, through redox cycle between Cu < 1 + > and Cu < 2 + >, active free radicals can be converted into oxygen-containing functional groups which are more stable on the surface of the PA6 composite material, and the oxygen-containing functional groups and amido bonds on a PA1012 chain in modified polyamide have hydrogen bond interaction, so that the thermal oxidation resistance, the impact resistance and the mechanical property of the hot melt adhesive can be enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hot melt adhesives, in particular to a method for preparing heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive. Background Art

[0002] Hot melt adhesive is an adhesive that is solid at room temperature and liquid after heating and melting. After applying it to the adherend, it can be bonded in a short time after pressing and cooling. Hot melt adhesive has the advantages of no chemical solvents, no pollution, easy to use and easy to store. Therefore, it has developed rapidly in recent years and its application fields have been continuously expanded. Among them, polyamide is the hot melt adhesive with the best bonding properties.

[0003] As an engineering polymer, polyamide has excellent heat resistance, cold resistance, electrical properties, and dielectric resistance. It can bond a variety of metals and non-metals and has good compatibility with other resins. It is used in many important fields, including electronic components, furniture, textiles, and coatings. However, polyamide is sensitive to oxygen and heat, and its mechanical properties will inevitably deteriorate during storage, transportation, and use. In order to reduce this effect, antioxidants are usually used during the molding process to reduce the thermal oxidation degradation rate of the material. At the same time, polyamide also has the disadvantages of low toughness and strong hydrophilicity, but researchers have discovered a simple melt co-condensation method to synthesize modified polyamides with different PA1012 salt contents, which show sufficient toughness. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot-melt adhesive to solve the problems raised in the background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A preparation method of a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive comprises the following steps: adding polyamide, modified polyamide and cuprous diethylphosphite into a mixer, raising the temperature to 180-250°C, stirring and mixing for 20-40 minutes, adding epoxy resin and zinc stearate, and continuing stirring for 20-50 minutes to obtain the heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive.

[0007] Furthermore, the mass ratio of the polyamide, modified polyamide, cuprous diethylphosphite, epoxy resin and zinc stearate is 100-150:40-120:5-15:5-20:2-8.

[0008] Further, the preparation method of the modified polyamide is as follows:

[0009] S1. In a nitrogen atmosphere, at 75° C., a mixture of 1,10-diaminodecane ethanol solution was added dropwise to a 1,10-decanedicarboxylic acid ethanol solution. After the addition was completed, the reaction mixture was stirred at 75° C. for another 6 h, the precipitate was filtered, and vacuum dried at 80° C. for 12 h to obtain PA1012 salt;

[0010] S2. Polymerization grade ε-caprolactam (CPL), PA1012 salt and deionized water are polymerized in a high-pressure reactor at a polymerization temperature of 240°C and a polymerization pressure of 0.4 MPa for 3 hours, and then the internal pressure of the reactor is gradually released to atmospheric pressure, and the reaction temperature is gradually heated to 250°C and maintained for 4 hours. In the final stage of the reaction, a flowing nitrogen atmosphere is maintained to discharge water in the condensation polymerization until the torque value reaches the target amount. The copolymer is extruded from the reactor, cooled, granulated, and extracted with superheated water to obtain a modified polyamide.

[0011] It should be noted that the polymerization process of modified polyamide mainly includes hydrolysis ring-opening polymerization of PA6 and melt polycondensation with different contents of PA1012 salt. Compared with PA6, the molecular chain of copolymer is more flexible and the chain segments are easier to move. When impacted, the impact energy can be dispersed into a larger volume and absorbed by the chain and converted into heat energy by the movement of the chain segments, so its impact resistance is improved.

[0012] Furthermore, in step S1, the mass fraction of the ethanol solution of 1,10-decanedicarboxylic acid is 98.7%; the mass fraction of the ethanol solution of 1,10-diaminodecane is 99.6%.

[0013] Furthermore, in step S1, the volume ratio of the ethanol solution of 1,10-decanedicarboxylic acid to the ethanol solution of 1,10-diaminodecane is 4-6:1-2.

[0014] Furthermore, in step S2, the mass ratio of CPL, PA1012 salt and deionized water is 45-50:250-300:1-2.

[0015] Furthermore, the preparation method of cuprous diethylphosphite is as follows: sodium diethylphosphinate (NaDP) is dissolved in DMF, then transferred to a three-necked flask equipped with a magnetic stirrer under a nitrogen flow, CuI is added, and stirring is continued at 80° C. for 12 hours. After filtering and washing three times with DMF, the product is dried at 80° C. for 12 hours to finally obtain cuprous diethylphosphite.

[0016] It should be noted that the presence of empty orbitals and variable valence states of Cu enables them and their oxides to exhibit excellent antioxidant activity in polymers through redox cycles between different valence states. Copper is highly reactive due to its empty electron orbitals, which can induce the esterification of polymers and form a protective barrier. At the same time, the release of PO·, HPO·, and HPO2· can capture free radicals (H·, OH·) and other active free radicals generated during the decomposition process, and the active free radicals can be converted into more stable oxygen-containing functional groups on the surface of PA6 composites.

[0017] Furthermore, the mass ratio of NaDP, DMF and CuI is 200-220:2-3:300-340.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The modified polyamide was synthesized by melt condensation of mixed CPL / 1012 salts. Compared with PA6, the molecular chain of the copolymer is more flexible and the chain segments are easier to move. When impacted, the impact energy can be dispersed into a larger volume and absorbed by the chain segment movement and converted into heat energy, so its impact resistance is improved. On the other hand, the spherulite size is too large, and the defects inside and between the spherulites increase, and the polymer is prone to break at the defects when impacted. After the introduction of long carbon chain PA1012, a decrease in crystallinity and spherulite size can be observed, and the energy dissipation during fracture is further increased, thereby improving the impact resistance of the modified polyamide.

[0020] (2) In the presence of heat and oxygen, the polymer generates active hydroperoxide (ROOH) + In the presence of Cu, ROOH undergoes a valence change to generate RO with lower activity. 1+ ions are oxidized to Cu 2+ , reducing the attack of free radicals on the fragile amide groups inside polyamide, destroying the degradation reaction. In addition, the introduction of electron-withdrawing metal cations has a strong interaction with the amide groups, resulting in uneven electron distribution, reducing the reactivity of the methylene groups close to the amide nitrogen, and inhibiting the formation of hydroperoxides.

[0021] (3) The polymer is heated and oxygenated by Cu 1+ and Cu 2+ Through the redox cycles, active free radicals can be converted into more stable oxygen-containing functional groups on the surface of PA6 composite materials. These oxygen-containing functional groups interact with the amide bonds on the PA1012 chains in the modified polyamide through hydrogen bonds, which can enhance the thermal oxidation resistance, impact resistance and mechanical properties of the hot melt adhesive. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The preparation method of modified polyamide is as follows:

[0024] S1. In a nitrogen atmosphere, at 75° C., a mixture of 206.8 g of 1,10-diaminodecane in 410 mL of ethanol solution was dropwise added to a solution of 259.5 g of 1,10-decanedicarboxylic acid in 1560 mL of ethanol. After the addition was complete, the reaction mixture was stirred at 75° C. for another 6 h, the precipitate was filtered, and vacuum dried at 80° C. for 12 h to obtain PA1012 salt;

[0025] S2. 110.3 g of CPL, 598.7 g of PA1012 salt and 15 L of deionized water were polymerized in a 30 L high-pressure reactor at a polymerization temperature of 240 ° C and a polymerization pressure of 0.4 MPa for 3 h, and then the internal pressure of the reactor was gradually released to atmospheric pressure, and the reaction temperature was gradually heated to 250 ° C and maintained for 4 h. In the final stage of the reaction, a flowing nitrogen atmosphere was maintained to discharge water in the condensation polymerization until the torque value reached the target amount, and the copolymer was extruded from the reactor, cooled, granulated, and extracted with superheated water to obtain the modified polyamide.

[0026] The preparation method of cuprous diethylphosphite is as follows: 206.4 mg of NaDP is dissolved in 1 mL of DMF, and then transferred to a 50 mL three-necked flask equipped with a magnetic stirrer under a nitrogen flow, 337.9 mg of CuI is added, and stirring is continued at 80° C. for 12 h. After filtering and washing three times with DMF, the product is dried at 80° C. for 12 h to finally obtain cuprous diethylphosphite.

[0027] Embodiment 1:

[0028] 20.5 g of polyamide, 5.8 g of modified polyamide, and 0.5 g of cuprous diethylphosphite were added to a mixer, the temperature was raised to 180° C., and the mixture was stirred for 30 min. Then, 4.0 g of epoxy resin and 1.5 g of zinc stearate were added, and the mixture was stirred for 40 min to obtain hot melt adhesive 1.

[0029] Embodiment 2:

[0030] 19.5 g of polyamide, 5.4 g of modified polyamide, and 0.4 g of cuprous diethylphosphite were added to a mixer, the temperature was raised to 190° C., and the mixture was stirred for 30 min. Then, 3.2 g of epoxy resin and 1.2 g of zinc stearate were added, and the mixture was stirred for 30 min to obtain hot melt adhesive 2.

[0031] Embodiment 3:

[0032] 25.1 g of polyamide, 6.9 g of modified polyamide, and 0.6 g of cuprous diethylphosphite were added to a mixer, the temperature was raised to 200° C., and the mixture was stirred for 25 min. Then, 4.0 g of epoxy resin and 1.5 g of zinc stearate were added thereto, and stirring was continued for 30 min to obtain hot melt adhesive 3.

[0033] Embodiment 4:

[0034] 24.9 g of polyamide, 5.2 g of modified polyamide, and 0.7 g of cuprous diethylphosphite were added to a mixer, the temperature was raised to 220° C., and the mixture was stirred for 40 min. Then, 3.9 g of epoxy resin and 1.3 g of zinc stearate were added, and the mixture was stirred for 50 min to obtain hot melt adhesive 4.

[0035] Comparative Example 1:

[0036] 20.5 g of polyamide, 4.2 g of modified polyamide, and 0.5 g of cuprous diethylphosphite were added to a mixer, the temperature was raised to 180° C., and the mixture was stirred for 30 min. Then, 4.0 g of epoxy resin and 1.5 g of zinc stearate were added, and the mixture was stirred for 40 min to obtain comparative hot melt adhesive 1.

[0037] Comparative Example 2:

[0038] 20.5 g of polyamide and 5.8 g of modified polyamide were added to a mixer, the temperature was raised to 180° C., and the mixture was stirred and mixed for 30 minutes. Then, 4.0 g of epoxy resin and 1.5 g of zinc stearate were added thereto, and stirring was continued for 40 minutes to obtain comparative hot melt adhesive 2.

[0039] Comparative Example 3:

[0040] 20.5 g of polyamide and 0.5 g of cuprous diethylphosphite were added to a mixer, the temperature was raised to 180° C., and the mixture was stirred for 30 min. Then, 4.0 g of epoxy resin and 1.5 g of zinc stearate were added, and the mixture was stirred for 40 min to obtain comparative hot melt adhesive 3.

[0041] Thermal oxidation degradation test: Place the sample in an oven at 180°C for thermal oxidation degradation test, and measure the time required for the sample to form a skin in the oven.

[0042] Impact test: Use an impact machine to measure the notched impact strength of the sample. The impact strength is calculated by dividing the recorded absorbed impact energy by the cross-sectional area of ​​the sample.

[0043] Mechanical properties test: Place the sample in a hot melt adhesive machine and melt it into a glue at 180°C. Use aluminum sheet as the adherend. After cooling, test the mechanical properties of the material.

[0044] The experimental data of the examples and comparative examples are shown in Table 1.

[0045] Table 1: Experimental test results of various embodiments and comparative examples

[0046]

[0047] Analysis shows that in the thermal oxidation degradation test, the time taken for the crusting to appear in Examples 1 to 4 and Comparative Examples 1 and 3 is longer, and the thermal oxidation resistance is better, while the time taken for Comparative Example 2 is shorter, and the thermal oxidation resistance is poor. This is because Examples 1 to 4 and Comparative Examples 1 and 3 contain cuprous diethylphosphite, while Comparative Example 2 does not contain cuprous diethylphosphite, so its thermal oxidation resistance is poor.

[0048] In the impact resistance experiment, Examples 1 to 4 and Comparative Example 1 have better impact resistance due to the presence of modified polyamide due to the effect of flexible long chains. In Comparative Example 2, the improvement in impact resistance brought by modified polyamide is not obvious. In Comparative Example 3, there is no modified polyamide and the impact resistance is poor.

[0049] In the test of mechanical properties, the mechanical properties of Examples 1 to 4 and Comparative Example 1 are improved compared with Comparative Example 2 and Comparative Example 3, but the improvement of mechanical properties of Comparative Example 1 is not obvious compared with Example 1. This is because the amount of modified polyamide incorporated is small and the interaction of hydrogen bonds is weakened, which is reflected in the decrease of elongation at break and tensile strength, the decrease of toughness, and the weakening of mechanical properties.

[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive, characterized in that: The following steps are involved: Add polyamide, modified polyamide and cuprous diethylphosphite into a mixer, heat up and stir to mix, then add epoxy resin and zinc stearate, continue stirring for 20-50 minutes to obtain heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive.

2. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 1, characterized in that: The heating, stirring and mixing temperature is 180-250° C. and the time is 20-40 minutes.

3. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 1, characterized in that: The mass ratio of the polyamide, modified polyamide, cuprous diethylphosphite, epoxy resin and zinc stearate is 100-150:40-120:5-15:5-20:2-8.

4. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 1, characterized in that: The preparation method of the modified polyamide is as follows: S1. In a nitrogen atmosphere, at 75° C., a mixture of 1,10-diaminodecane ethanol solution was added dropwise to a 1,10-decanedicarboxylic acid ethanol solution. After the addition was completed, the reaction mixture was stirred at 75° C. for another 6 h, the precipitate was filtered, and vacuum dried at 80° C. for 12 h to obtain PA1012 salt; S2. CPL, PA1012 salt and deionized water are polymerized in a high-pressure reactor at a polymerization temperature of 240°C and a polymerization pressure of 0.4 MPa for 3 hours, and then the internal pressure of the reactor is gradually released to atmospheric pressure, and the reaction temperature is gradually heated to 250°C and maintained for 4 hours. In the final stage of the reaction, a flowing nitrogen atmosphere is maintained to discharge water in the condensation polymerization until the torque value reaches the target amount. The copolymer is extruded from the reactor, cooled, granulated, and extracted with superheated water to obtain the modified polyamide.

5. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 4, characterized in that: In step S1, the mass fraction of the ethanol solution of 1,10-decanedicarboxylic acid is 98.7%; the mass fraction of the ethanol solution of 1,10-diaminodecane is 99.6%.

6. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 4, characterized in that: In step S1, the volume ratio of the ethanol solution of 1,10-decanedicarboxylic acid to the ethanol solution of 1,10-diaminodecane is 4-6:1-2.

7. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 4, characterized in that: The mass ratio of CPL, PA1012 salt and deionized water in step S2 is 45-50:250-300:1-2.

8. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 1, characterized in that: The preparation method of cuprous diethylphosphite is as follows: NaDP is dissolved in DMF, and then transferred to a three-necked flask equipped with a magnetic stirrer under a nitrogen flow, CuI is added, and stirring is continued at 80° C. for 12 hours. After filtering and washing three times with DMF, the product is dried at 80° C. for 12 hours to finally obtain cuprous diethylphosphite.

9. The method for preparing a heat-resistant, oxidation-resistant and impact-resistant polyamide hot melt adhesive according to claim 8, characterized in that: The mass ratio of NaDP, DMF and CuI is 200-220:2-3:300-340.