Biomass composite phase change energy storage material and preparation method thereof

Through acid leaching and high-temperature calcination, the biomass porous materials adsorb phase change materials and wraps epoxy resin, the problems of leakage of phase change materials and low utilization efficiency of biomass materials are solved, and high thermal conductivity, low cost and environmental protection are achieved Preparation of composite phase change energy storage materials.

CN118931498APending Publication Date: 2024-11-12NINGBO UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410889009.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing phase change materials are prone to leakage during solid-liquid phase transformation, which affects energy storage efficiency and may cause environmental pollution. Moreover, the preparation process of biomass support materials is complex, has high cost and is very polluted, making it difficult to effectively utilize agricultural biowaste.

Method used

Using acid leaching and high-temperature calcination as a carrier, the phase change material is adsorbed by vacuum impregnation and epoxy resin is wrapped on the surface to prepare a biomass composite phase change energy storage material with high thermal conductivity to reduce leakage Risk and realize resource recycling and reuse.

Benefits of technology

The thermal conductivity and energy storage density of phase change materials are improved, production costs are reduced, agricultural biowaste is effectively utilized, environmental pollution is reduced, and pores are closed through epoxy resin, enhancing the thermal reliability of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931498A_ABST
    Figure CN118931498A_ABST
Patent Text Reader

Abstract

The invention discloses a biomass composite phase change energy storage material which comprises a phase change material and a biomass carrier matrix, the phase change material is adsorbed in pores of the biomass carrier matrix, and the biomass carrier matrix is a biomass porous material obtained by carrying out acid leaching treatment and high-temperature calcination on a biomass material. The surface of the biomass carrier matrix adsorbed with the phase change material can also be wrapped with epoxy resin. The biomass material is treated into the porous material by adopting acid leaching treatment and high-temperature calcination, so that the adsorption of the phase change material is facilitated. The phase-change material is dispersed and fixed in pores of the biomass material through vacuum adsorption, the heat conduction efficiency of the phase-change material is increased by taking a structure rich in the biomass material as a cross-linked network base in the heat storage material, and the energy storage material with good and stable heat storage performance is prepared and can be used for heat preservation of building walls.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials and energy recycling, and in particular to a method for preparing a composite phase change energy storage material by using biomass materials and phase change materials. Background Art

[0003] It is urgent to use new materials and technologies to improve the quality of rural housing construction, improve the rural indoor thermal environment, and reduce building energy consumption. Phase change materials, as a highly potential thermal energy storage technology, are increasingly widely used in the future construction industry. Phase change enclosure structures have the function of improving the thermal performance of walls and improving indoor thermal comfort.

[0004] Phase change materials are materials that absorb or release a large amount of latent heat by changing phases (such as from solid to liquid or from liquid to gas) at a specific temperature, thus having significant application advantages in temperature regulation, thermal energy storage and energy supply. The process of changing physical properties is called phase change, during which phase change materials will absorb or release a large amount of latent heat. Due to the phase change heat storage characteristics, phase change materials are currently widely used in aviation, construction, refrigeration, communications, electricity and other industries.

[0005] However, when the phase change material changes from solid to liquid, some of the material may escape in liquid form, which is called "leakage". This is especially common in organic phase change materials because their volume expands when they melt, and if they are not properly packaged, it may cause material leakage. Leakage will not only lead to a reduction in the amount of material and affect the energy storage efficiency, but may also pollute the environment or damage the equipment due to the overflow of the material. In order to avoid leakage problems, the phase change material can be confined to a certain space through packaging technology, or porous support materials can be used for load adsorption, thereby reducing or avoiding the occurrence of leakage.

[0006] Loading phase change materials onto suitable porous support materials to prepare composite phase change materials can enhance the heat transfer efficiency of the heat storage and release process, and can effectively solve the leakage and corrosion problems of the liquid phase during the solid-liquid phase transition of the phase change material. It is a hot topic in the research of phase change energy storage materials.

[0007] The supporting materials of composite phase change materials are mostly derived from petroleum derivatives, which have problems such as complex preparation process, high cost and high pollution. Bio-based supporting materials are a good solution, and their application prospects are broad due to their degradability and renewability.

[0008] Biomass materials are lumps made of biomass waste. Currently, biomass waste is generally used for landfill, composting, incineration and other fields, with low utilization efficiency. Large amounts of biomass materials piled up in the open air will also pollute the environment. How to effectively solve the defects of phase change materials and the problem that biomass materials are prone to waste resources and environmental pollution has become a difficult problem that technicians need to overcome. Summary of the invention

[0009] In order to solve the problems existing in the prior art, on the first aspect, the present invention provides a biomass composite phase change energy storage material with high thermal conductivity prepared by using biomass materials and phase change materials; on the second aspect, the present invention provides a method for preparing a biomass composite phase change energy storage material with high thermal conductivity by using biomass materials and phase change materials, which method can reduce agricultural biological waste and realize resource recycling and reuse.

[0010] The technical solution adopted by the present invention is specifically as follows:

[0011] A biomass composite phase change energy storage material comprises a phase change material and a biomass carrier matrix. The phase change material is adsorbed in the pores of the biomass carrier matrix. The biomass carrier matrix is ​​a biomass porous material obtained by acid leaching and high-temperature calcination of the biomass material.

[0012] Furthermore, the biomass material is agricultural waste biomass material, and preferably the biomass material is a mixture of one or more of rice husk, straw, lignin and chitin.

[0013] The phase change material includes a mixture of one or more of caprylic acid, capric acid, lauric acid, palmitic acid, myristic acid, stearic acid, myristyl alcohol, palmityl alcohol, stearyl alcohol, octadecane, and paraffin.

[0014] Furthermore, the mass ratio of the phase change material to the biomass carrier matrix is ​​1:0.1-2, preferably 1:0.1-1.

[0015] The biomass composite phase change energy storage material may further include epoxy resin, and the epoxy resin is wrapped on the surface of the biomass carrier matrix adsorbed with the phase change material.

[0016] Furthermore, the mass ratio of the phase change material, the biomass carrier matrix, and the epoxy resin is 1:0.1~1:0.1~1.

[0017] The present invention also provides a method for preparing the biomass composite phase change energy storage material, which comprises the following steps:

[0018] 1) The biomass material is sequentially subjected to acid leaching, high temperature calcination, and crushing to obtain biomass powder;

[0019] 2) Biomass powder is used as a carrier, a phase change material is loaded by a vacuum impregnation method, and then the surface is coated with epoxy resin to obtain the biomass composite phase change energy storage material.

[0020] Furthermore, in step 1), the crushed powder is sieved through a 10-mesh sieve to obtain biomass powder.

[0021] Furthermore, in step 1), the step of acid leaching treatment of the biomass material is as follows: the biomass material is immersed in an acidic solution for 1 to 24 hours (preferably 1 to 5 hours), the concentration of the acidic solution is 0.1 to 1.3 mol / L (preferably 0.2 to 0.5 mol / L), and the acidic solution is sulfuric acid, hydrochloric acid, nitric acid, citric acid, acetic acid or carbonic acid, preferably citric acid.

[0022] Citric acid is an organic acid. Organic acids usually have weak acidity and can form stable chelates with metal ions, which helps to remove metal impurities from rice husks. It is more environmentally friendly than inorganic acids. The acidic organic mixed solution after the reaction of citric acid and metal ions is easily degraded by low-energy anaerobic microbial treatment technology, which meets the requirements of green chemistry. The hydroxyl and carboxyl functional groups in the molecular structure of citric acid can react with metal ions in rice husks to form stable liquid polycyclic metal chelates, thereby effectively removing metal elements.

[0023] Preferably, the immersion temperature is 40-60°C, more preferably 50°C.

[0024] More preferably, after immersion, the biomass material is filtered and washed, and the solid product is dried to obtain an acid-leached biomass material;

[0025] The mass ratio of the biomass material to the acidic solution is preferably 1:10-50.

[0026] Drying is generally carried out at 90-95°C for 10-15 hours.

[0027] The acid-leached biomass material is subjected to high-temperature calcination, and the high-temperature calcination step is preferably one of the following:

[0028] (a) calcining at 500-700° C. (preferably 650-680° C.) in an air environment for 2-3 h;

[0029] (b) calcining at 400-450° C. for 1-2 h in an inert gas environment, and further heating to 600-900° C. (preferably 800-850° C.) for 1-3 h.

[0030] The inert gas is argon, nitrogen, helium or krypton, preferably nitrogen.

[0031] Step (a) is calcined in air environment to obtain silica-based powder, which is recorded as rice husk-based silicon RHS.

[0032] Step (b) is calcined under an inert gas environment to obtain high temperature carbonized rice husk charcoal, which can be recorded as RHC.

[0033] In the step 2), the steps of the vacuum impregnation method are:

[0034] Biomass powder is used as a carrier, air is removed by vacuuming, and then the heated and melted phase change material is added, the temperature is maintained at 50-70°C, and the mixture is stirred and mixed evenly. Under a vacuum environment, the phase change material is adsorbed and filled into the pores of the carrier matrix to obtain a composite phase change energy storage material;

[0035] The vacuuming to remove air can generally be maintained at an absolute pressure of 50 to 100 kPa for 2 hours.

[0036] The vacuum environment preferably has an absolute pressure of 0 to 0.1 MPa, preferably 0.05 to 0.09 MPa, and a temperature of 50 to 70°C.

[0037] The adsorption time is preferably 6 to 8 hours.

[0038] Furthermore, the vacuum impregnation method is preferably operated according to the following steps: in a vacuum environment, the phase change material is adsorbed and filled into the pores of the carrier matrix, which can be operated according to the following steps:

[0039] Biomass powder is used as a carrier, and air is removed by vacuuming. Then, the heated and melted phase change material is added, and the temperature is maintained at 50-70°C (preferably 60-70°C). The mixture is stirred and mixed evenly. Air is introduced until atmospheric pressure is reached. After sufficient stirring and mixing, the mixture is vacuumed to 0.05-0.09MPa. The temperature is maintained at 50-70°C (preferably 60-70°C). The mixture is vacuumed for 6-8h, and air is introduced to normal pressure. The mixture is stirred and mixed to obtain a composite phase change energy storage material.

[0040] The surface of the composite phase change energy storage material is coated with epoxy resin, and generally the temperature is kept at 60-65°C, epoxy resin is added, mixed and then cooled to obtain a biomass composite phase change energy storage material.

[0041] Furthermore, in step 2), the mass ratio of phase change material to biomass powder is 1:0.5-2.

[0042] Furthermore, in step 2), the mass ratio of phase change material, biomass powder and epoxy resin is 1:0.1~1:0.1~1.

[0043] During the cooling in step 2), a mold can be used to mold the product to obtain a finished product, and the molding time is usually 24 hours.

[0044] The biomass composite phase-change energy storage material provided by the present invention can be used for thermal insulation of building walls.

[0045] The whole preparation process of the present invention uses biomass materials and phase change materials to prepare biomass composite phase change energy storage materials. First, the biomass materials are treated into porous materials by chemical methods. The biomass-derived carbon materials usually show structural diversity, including spherical, fibrous, layered and 3D structures. The carbonized biomass contains a large number of mesopores and macropores, which are conducive to the adsorption of phase change materials. The phase change material is dispersed and fixed in the pores of the biomass material by vacuum adsorption, and the structure rich in the biomass material is used as the cross-linked network base in the heat storage material to increase the thermal conductivity of the phase change material, so as to prepare a stable energy storage material with good heat storage performance. The rice husk powder used in the present invention is a very rich waste resource, which is not only low in price, but also can reduce the pollution of agricultural biological waste to the environment while realizing resource recycling and reuse.

[0046] The beneficial effects of the present invention include at least:

[0047] 1. The present invention uses rice husks as biomass materials obtained by different preparation methods to prepare energy storage material substrates, which can improve the thermal conductivity of phase change materials and increase the energy storage density of energy storage materials.

[0048] 2. The present invention uses waste biomass materials for preparation, which can reduce the production cost of high-performance energy storage materials, directly and effectively utilize the loose porous structure in the waste biomass materials, and facilitate the recovery of phase change materials.

[0049] 3. The present invention uses waste biomass to prepare energy storage materials, which can efficiently utilize waste resources, and play a role in energy conservation, environmental protection and waste resource recycling.

[0050] 4. Use epoxy resin to wrap the biomass composite phase change energy storage material to seal the pores, further prevent the leakage of the phase change material, and shape the composite phase change material to reduce the fluidity of the phase change material, further improving the thermal reliability of the composite material.

[0051] 5. The preparation method of the present invention is simple. The acid leaching modification treatment of rice husk can effectively remove impurities and has little effect on the structure of rice husk. The biomass carrier prepared by acid leaching treatment and high-temperature calcination has better adsorption. Compared with general energy storage materials, the biomass composite phase change energy storage material prepared by the present invention has the advantages of low cost, high heat storage performance, and low phase separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 These are scanning electron microscope images (SEM) of biomass carriers and composite phase change materials, (a) is the SEM image of RHS, (b) is the SEM image of n-octadecane / RHS composite phase change material, (c) is the SEM image of RHC, and (d) is the SEM image of n-octadecane / RHC composite phase change material.

[0053] Figure 2 : The Fourier transform infrared spectra of the biomass carrier and the composite phase change material, wherein (a) is the Fourier transform infrared spectra of RHS, n-octadecane and n-octadecane / RHS; (b) is the Fourier transform infrared spectra of RHC, n-octadecane and n-octadecane / RHC.

[0054] Figure 3 1 and 1 are thermal performance test results of octadecane, octadecane / RHS, and octadecane / RHC, where (a) is a DSC curve and (b) is a comparison chart of melting enthalpy and solidification enthalpy.

[0055] Figure 4 It is a comparative bar chart of the thermal conductivity of octadecane, octadecane / RHS, and octadecane / RHC. DETAILED DESCRIPTION

[0056] The present invention will be described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form.

[0057] It should be pointed out that, for those skilled in the art, several changes and improvements can be made without departing from the concept of the present invention, including any combination of various examples.

[0058] Example 1

[0059] The high-performance biomass composite phase-change energy storage material produced by the present invention uses waste biomass materials and octadecane materials with a melting point of 28-31° C. The specific preparation method is as follows:

[0060] (1) Rice husk-based silica (RHS) was prepared using a citric acid soaking and high-temperature calcination treatment method. 25 g of rice husk powder was leached in a 5 wt% citric acid solution (500 mL) at 50°C for 2 h. The solution was then filtered and the rice husk powder was washed three times with deionized water. Then, it was dried in an oven at 90°C for 12 h. Finally, the modified rice husk powder was annealed in an air atmosphere (muffle furnace) at 650°C for 2 h. The final product consisted of silica-based powder, recorded as rice husk-based silicon RHS. The yield of silica-based powder extracted from rice husk was about 10.9%. The silica-based powder had a nearly white appearance.

[0061] (2) Rice husk-based charcoal (RHC) was prepared using citric acid soaking and high-temperature pyrolysis. The specific procedure included leaching 25 g of rice husk powder in a 5 wt% citric acid solution (500 mL) at 50 °C for 2 h. The solution was then filtered and the rice husk powder was washed three times with deionized water. Then, it was dried in an oven at 90 °C for 12 h. Finally, the modified rice husk powder was placed in a quartz boat and heated to 400 °C in a tubular furnace in a nitrogen environment (nitrogen flow rate of 8 m / s) at a heating rate of 10 °C / min, and then pyrolyzed at 400 °C for 1 h. Subsequently, the pyrolyzed material was heated to 800 °C under the same atmospheric conditions and kept at 800 °C for 2 h. High-temperature carbonized rice husk charcoal (RHC) was obtained.

[0062] The pore size distribution of silicon-based and carbon-based biomass porous materials made from rice husks is shown in Table 1:

[0063] Table 1 Pore size distribution of silicon-based and carbon-based biomass porous materials made from rice husk

[0064]

[0065] Different pore structures have a great influence on the crystallization behavior and thermal stability of porous materials. Table 1 summarizes the N2 physical adsorption data of RHS and RHC. According to the IUPAC (mesopores between 2nm and 50nm) adsorption isotherm, RHS belongs to type IV isotherm and RHC also belongs to type IV isotherm. This is due to the relatively strong interaction between the adsorbent material and the adsorbed gas. At higher relative pressures, RHC will have an inflection point, which indicates that the molecular clusters are filled with pores. Pore size distribution is one of the important factors for RHS and RHC as PCM support materials. As shown in Table 1, the BET surface area of ​​RHS is 188m 2 / g, average pore diameter of 6.1nm, total pore volume of 290mm 3 / g; the BET surface area of ​​RHC is 20.1m 2 / g, average pore diameter is 2.9nm, total pore volume is 36.2mm 3 / g. The large specific surface area and rich mesoporous structure are conducive to the adsorption of a large amount of phase change materials, improving the thermal reliability of n-octadecane / RHS and n-octadecane / RHC composites during the melting and solidification phase change cycle. For the composite phase change material samples, due to the impregnation of a large amount of phase change materials, the composite materials are severely agglomerated, and their BET specific surface area and pore volume are much smaller than those of RHS and RHC, and even cannot be measured by instruments.

[0066] (3) n-octadecane / RHS and n-octadecane / RHC composite phase change materials were synthesized by vacuum impregnation. The supporting matrix carrier (RHS or RHC) was placed in a flask connected to a vacuum pump, and the air was completely removed by applying an absolute air pressure of 64 kPa for 2 hours. Then, the molten n-octadecane was gradually added to the supporting matrix carrier, the temperature was kept above 60°C, and the mixture was stirred and mixed evenly. After that, the vacuum was released, the air flow rate was kept at 10-20 m / s, and stirring was maintained to promote the penetration of liquid n-octadecane into RHS or RHC until the pressure reached 101 kPa. After mixing evenly, vacuum was drawn again, the temperature was kept above 60°C, and vacuum adsorption was performed for 6-8 hours at an absolute pressure of 0.05-0.09 MPa. Finally, epoxy resin was added at a temperature of 60-65°C to enhance its anti-leakage performance, and composite phase change materials octadecane / RHS and octadecane / RHC were obtained.

[0067] The above step (3) is specifically as follows:

[0068] According to the mass ratio of N-octadecane: rice husk ash silicon-based biomass carrier: epoxy resin of 5:5:2; N-octadecane: rice husk ash carbon-based biomass carrier: epoxy resin of 5:2:2, take the dried carrier matrix, octadecane and the corresponding epoxy resin, preheat the octadecane to 60°C, so that the octadecane is in a completely melted state. The dried carrier matrix is ​​placed in a flask, and the flask is placed in a 60°C constant temperature water bath. The air is completely removed under a vacuum pressure of 64kPa for 2h. The melted octadecane is poured into the dropping funnel, the funnel valve is opened, and the octadecane is dripped onto the carrier matrix and then air is added until atmospheric pressure is reached. Mechanical stirring is performed for 40min, the temperature of the molten mixture is kept above 65°C, and ultrasonic stirring is performed for 25min, and then it is placed in a constant temperature vacuum drying oven, the pressure is set to 0.08Mpa, the temperature is maintained at 65°C, and adsorption is performed under this condition for 6h. Air is introduced to normal pressure to obtain a uniformly mixed composite phase change material. The adsorbed composite material is kept at 60°C, and a corresponding amount of epoxy resin is added and stirred thoroughly. Then, the mold is made at room temperature for 24 hours. The finished biomass material-octadecane composite phase change energy storage material is obtained, which is recorded as composite phase change material octadecane / RHS and octadecane / RHC, i.e., biomass composite phase change energy storage material.

[0069] Figure 1The scanning electron microscope images in the figure show the successful loading of octadecane on the carbon-based and silicon-based substrates of rice husk ash. From the scanning electron microscope images of the carbon-based and silicon-based substrates of rice husk ash in Figures (a) and (c), it can be observed that there are a large number of pores on the carbon / silicon-based substrates of rice husk ash. These pores provide sufficient space for octadecane. As shown in Figures (b) and (d), the pores in the carbon / silicon-based substrates of rice husk ash are filled with a large number of spherical octadecane particles. The size of the octadecane particles is about a few microns. The small particles increase the thermal surface area of ​​octadecane, which is beneficial for heat transfer.

[0070] The FT-IR spectra of n-octadecane / RHS and n-octadecane / RHC composite PCMs are shown in Figure 2. Figure 2 (a) and (b). Usually, at about 3400cm -1 The broad peak at 2918 cm is mainly due to the stretching vibration of the OH group in the adsorbed H2O molecules. -1 and 2847cm -1 The characteristic absorption peak at 1470 cm is the stretching vibration of -CH2. -1 The characteristic absorption peak at 717cm is the asymmetric bending vibration of -CH3. -1 The peak at 7992cm represents the deformation vibration and rocking vibration of the -CH2 matrix. -1 and 1042cm -1 The RHC peaks at correspond to Si-O-Si symmetric and asymmetric stretching vibrations, respectively. In the FT-IR spectra of RHS and the prepared n-octadecane / RHS composite PCMs, no obvious peaks were found except for the characteristics of n-octadecane and RHS; this indicates that no chemical bonds were formed between the porous RHS and n-octadecane. Figure 2 As shown in (b), the FT-IR spectrum of RHC does not show obvious vibration characteristics unique to carbon-based materials. However, the stretching vibration of Si-O-Si can still be observed in the infrared spectrum of RHC, and its peak intensity is weaker than that of RHS. This is mainly due to the high carbon content present in biochar. Unlike n-octadecane / RHS, the characteristic peak intensity of n-octadecane / RHC increases slightly and shifts to lower wavenumbers due to the effect of carbon-based support materials on the thermal properties of encapsulated n-octadecane. In addition, no new characteristic peaks were observed in the n-octadecane / RHC spectrum, nor was the disappearance of old characteristic peaks. The results show that there is no chemical bond between n-octadecane and RHC; there is only a physical force between them, indicating that they have good chemical compatibility.

[0071] The thermal stability of octadecane, octadecane / RHS, and octadecane / RHC was tested by placing the filter paper on a constant temperature plate at 65°C, placing the material on the filter paper, and observing whether the filter paper was soaked. The results showed that after heating octadecane for 1 minute, the filter paper had a large area of ​​liquid leakage, while after heating the composite materials octadecane / RHS and octadecane / RHC for 10 minutes, there was almost no leakage on the filter paper.

[0072] Thermal performance test

[0073] Test method: Weigh about 5 mg of phase change material octadecane and biomass-based phase change latent heat storage materials octadecane / RHS and octadecane / RHC and place them in a crucible, and take an empty crucible as a reference sample. Set the N2 gas flow in the DSC test to 50 ml / min, increase the temperature from 10°C to 80°C at a heating rate of 10°C / min, and then cool it from 80°C to 10°C at a cooling rate of 10°C / min.

[0074] The thermal conductivity was tested using the transient plate heat source method (instrument: TPS2500S). The results are as follows: Figure 4 shown.

[0075] Results analysis: In the process of heating and cooling, the phase change material has a certain ability to store and release heat. The thermal enthalpy value can indicate the heat storage capacity of the composite phase change material. The DSC curves of octadecane and biomass-based phase change latent heat storage materials and the corresponding thermal performance data are shown in Figure 2. Figure 3 As shown in Table 2. The melting and crystallization temperatures of rice husk silicon-based phase change composites are around 26°C and 25°C, respectively, and the melting and crystallization temperatures of rice husk carbon-based phase change composites are around 27°C and 26°C, respectively. Biomass-based porous carbon materials have a certain influence on the melting and crystallization process of phase change materials. It can be seen that the supercooling of rice husk phase change composites is smaller than that of pure phase change materials.

[0076] The shape of the DSC curve of the biomass-based porous carbon material does not change much after 300 hot and cold cycles, indicating that the prepared composite phase change material has excellent thermal reliability.

[0077] Table 2 Performance test results of biomass-based phase change latent heat storage materials

[0078]

[0079] According to the experiment, the melting enthalpy of rice husk silicon-based composite phase change energy storage material is 106.5J / g, the phase change temperature is 26.5℃, and its thermal conductivity ( Figure 4 The thermal conductivity of rice husk carbon-based composite phase change energy storage material is 2.25 times higher than that of pure octadecane; the melting enthalpy (latent heat of phase change enthalpy value) of rice husk carbon-based composite phase change energy storage material is 116.3 J / g, the phase change temperature is 27.7°C, and its thermal conductivity is 1.56 times higher than that of pure octadecane.

[0080] Comparative Example

[0081] The rice husk powder in step (1) of Example 1 was replaced with equal amounts of lignin and chitosan to prepare lignin-based silica and chitosan-based silica, respectively.

[0082] The rice husk powder in step (2) of Example 1 was replaced with equal amounts of lignin and chitosan to prepare lignin-based charcoal and chitosan-based charcoal, respectively.

[0083] Lignin-based silica, chitosan-based silica, lignin-based charcoal and chitosan-based charcoal are bio-based carrier matrices. Octadecane is adsorbed by vacuum impregnation according to the method of step (3), and epoxy resin is coated on the surface to obtain four composite phase change materials: octadecane / lignin-based silica, octadecane / chitosan-based silica, octadecane / lignin-based charcoal and octadecane / chitosan-based charcoal.

[0084] The thermal stability of the four composite phase change materials was tested by placing the filter paper on a constant temperature plate at 65°C, placing the material on the filter paper, and observing whether the filter paper was soaked. The results showed that the four composite materials had liquid leakage on the filter paper after heating for 5 minutes. The rice husk powder used in Example 1 had a more outstanding anti-leakage performance.

[0085] The above is only a preferred embodiment of the present application, and is not any formal or substantial limitation to the present application. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present application, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present application, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present application; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the substantial technology of the present application are still within the scope of the technical solution of the present application.

Claims

1. A biomass composite phase change energy storage material, characterized in that: The biomass composite phase change energy storage material comprises a phase change material and a biomass carrier matrix, the phase change material is adsorbed in the pores of the biomass carrier matrix, and the biomass carrier matrix is ​​a biomass porous material obtained by acid leaching and high-temperature calcination of the biomass material.

2. The biomass composite phase change energy storage material according to claim 1, characterized in that: The biomass material is a mixture of one or more of rice husk, straw, lignin and chitin; The phase change material includes a mixture of one or more of caprylic acid, capric acid, lauric acid, palmitic acid, myristic acid, stearic acid, myristyl alcohol, palmityl alcohol, stearyl alcohol, octadecane, and paraffin.

3. The biomass composite phase change energy storage material according to claim 1, characterized in that: The biomass composite phase change energy storage material also includes epoxy resin, and the epoxy resin is wrapped on the surface of the biomass carrier matrix adsorbed with the phase change material.

4. The biomass composite phase change energy storage material according to claim 3, characterized in that: The mass ratio of the phase change material, the biomass carrier matrix and the epoxy resin is 1:0.1-1:0.1-1.

5. The method for preparing the biomass composite phase change energy storage material according to claim 3 or 4, characterized in that: The method comprises the following steps: 1) The biomass material is sequentially subjected to acid leaching, high temperature calcination, and crushing to obtain biomass powder; 2) Biomass powder is used as a carrier, a phase change material is loaded by a vacuum impregnation method, and then the surface is coated with epoxy resin to obtain the biomass composite phase change energy storage material.

6. The method according to claim 5, characterized in that In step 1), the steps of acid leaching treatment of biomass material are: The biomass material is immersed in an acidic solution for 1 to 24 hours, the concentration of the acidic solution is 0.1 to 1.3 mol / L, and the acidic solution is sulfuric acid, hydrochloric acid, nitric acid, citric acid, acetic acid or carbonic acid.

7. The method according to claim 5, characterized in that In step 1), the high temperature calcination step is one of the following: (a) Calcination at 500-700°C for 2-3h in air environment; (b) calcining at 400-450°C for 1-2 h in an inert gas environment, and further heating to 600-900°C for calcining for 1-3 h.

8. The method according to claim 5, characterized in that In the step 2), the steps of the vacuum impregnation method are: Biomass powder is used as a carrier, and air is removed by vacuuming. Then, the heated and melted phase change material is added, and the temperature is maintained at 50-70°C. The mixture is stirred and mixed evenly. Under a vacuum environment, the phase change material is adsorbed and filled into the pores of the carrier matrix to obtain a composite phase change energy storage material.

9. The method according to claim 8, characterized in that The absolute pressure of the vacuum environment is 0.05-0.09 MPa, the temperature is maintained at 50-70° C., and the adsorption time is 6-8 hours.

10. Use of the biomass composite phase change energy storage material according to any one of claims 1 to 4 in building wall insulation.