Phase change energy storage material with copper slag core-shell structure and preparation method of phase change energy storage material
Through the design of the copper slag core shell structure, the corrosion and leakage problems caused by porous alumina ceramic shell are solved, the stability and thermal conductivity of energy storage materials are improved, and the sensible heat storage capacity and efficient utilization of resources are achieved.
Patent Information
- Application Number
- CN202411002198.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
The existing alumina ceramic shells are porous after sintering, resulting in corrosion and leakage of energy storage materials, and insufficient sealing properties, affecting heat storage performance.
The copper slag core-shell structure is adopted, solid aluminum spheres are used as the core, and copper slag mixed ceramic powder is used as the cladding layer. The cavity is discharged by heating the solid alkane compound, and copper slag is added to form Fe2O3, enhancing the stability and thermal conductivity of the material.
It significantly improves the stability and thermal conductivity of the material, prevents corrosion and leakage, enhances the ability to store heat in sensible heat, and realizes the high-value utilization of resources.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of phase change energy storage material synthesis, and specifically relates to a copper slag core-shell structure phase change energy storage material and a preparation method thereof. Background Art
[0002] As energy demand continues to increase, developing efficient and clean energy systems has become a global urgent task. Currently, more than 90% of the world's primary energy generation is achieved through thermal energy consumption or waste. Thermal energy plays a wide and important role in efficient and sustainable energy utilization. The development of efficient thermal energy storage systems using thermal storage materials can solve the problem of energy supply and demand mismatch and alleviate the depletion of fossil resources.
[0003] Core-shell energy storage materials are a class of materials with a special structure, usually consisting of a core and a cladding layer. However, the current alumina ceramic shell is still porous after sintering, which leads to two key problems that reduce the performance of energy storage materials: on the one hand, the porous shell allows external air to flow into the core and react with the metal during thermal cycling, causing core corrosion. On the other hand, the sealing of the cladding layer is insufficient, and molten metal or metal vapor flows out through the porous shell, causing leakage.
[0004] The present invention proposes a new energy storage material, which uses a solid aluminum ball as the core and copper slag mixed ceramic powder as the coating layer. The cavity between the core and the coating layer is the cavity after the solid alkane compound is heated and discharged. This structure is designed to adapt to the thermal expansion of Si-Al, and by adding copper slag to the shell, Fe 2 O 3 To improve the stability of the material. At the same time, the design also enhances the material's heat storage capacity and thermal conductivity. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] The present invention aims to solve the leakage and corrosion problems of packaging materials and improve the sensible heat storage capacity of the finished product on this basis. To this end, a copper slag core-shell structure phase change energy storage material and a preparation method thereof are proposed, which have both excellent stability and good sensible heat storage capacity and a preparation method thereof.
[0007] (II) Technical solution
[0008] To achieve the above object, the present invention provides a copper slag core-shell structure phase change energy storage material and a preparation method thereof, comprising a technical solution adopting the following steps:
[0009] Step 1, temporary composite core preparation
[0010] The sacrificial solid alkane mixture is evenly coated on the surface of the aluminum ball by a rotary coater to form a shell to obtain the required temporary composite core, and the particle size range is 19 to 22 mm.
[0011] The solid alkane mixture is petrolatum, and the coating thickness is 1 to 2 mm.
[0012] The spin coater is a stainless steel cavity heating glue spreader.
[0013] The aluminum ball is a common industrial aluminum ball with a diameter of 18 to 20 mm. 2 O 3 The purity is more than 90%.
[0014] Step 2: Shell preparation
[0015] 1) Preparation of inner shell: A mixed ceramic powder without copper slag is evenly applied on the prepared temporary composite core by a rotary coater to obtain an inner shell.
[0016] 2) Shell preparation: Mixed ceramic powder containing copper slag is coated on a single-layer shell to make a double-layer shell material.
[0017] The ceramic is common alumina ceramic.
[0018] The mixing ratio of the mixed ceramic powder is: 0-30% copper slag; 6% cement binder; Al 2 O 3 Powder 5%; Kyanite powder 7%; Silica powder 1%; Bauxite 50-80%.
[0019] The mixed ceramic powder is applied with a thickness of 1 to 1.5 mm.
[0020] Step 3: Drying, sintering, cooling
[0021] The prepared spheres are placed in an oven at 80-100° C. to dry for 6-12 hours, and then heated in a box furnace at 1000-1200° C. to sinter them, and the final material is obtained after cooling to room temperature.
[0022] The sintering is carried out under vacuum conditions, and the heat preservation time is 2 to 3 hours.
[0023] (III) Beneficial effects
[0024] The present invention provides a copper slag core-shell structure phase change energy storage material and a preparation method thereof, which has the following beneficial effects:
[0025] 1. Resource utilization: The energy storage material provided by the present invention is mainly prepared from aluminum balls, solid alkane mixture, copper slag and mixed ceramic powder, which realizes the resource utilization of solid waste and provides a new technical idea for the high-value utilization of copper slag.
[0026] 2. Improved sensible heat storage capacity and thermal conductivity: The present invention significantly improves the sensible heat storage capacity and thermal conductivity of the material, while enhancing the stability of the material. After the cycle test, the material weight increased less, showing excellent cycle stability.
[0027] 3. Enhanced shell stability and sealing: The addition of copper slag allows the shell to generate Fe2O3 during the cycle, further improving the stability of the material. At the same time, the double-layer shell structure effectively blocks the entry of air, thereby preventing corrosion of the internal material and preventing leakage of molten metal. This design effectively solves the corrosion and leakage problems faced by phase change energy storage materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The following is a flow chart of material preparation. The specific preparation steps and instructions are as follows:
[0029] S1: The solid alkane mixture is evenly applied on the surface of the aluminum ball by a rotary coater to form a shell to obtain the required temporary composite core, and the particle size range is 19 to 22 mm.
[0030] S2: 1) Preparation of inner shell: Using a rotary coater, a mixed ceramic powder without copper slag is evenly applied on the prepared temporary composite core to obtain an inner shell.
[0031] 2) Shell preparation: Mixed ceramic powder containing copper slag is coated on a single-layer shell to make a double-layer shell material.
[0032] S3: The prepared spheres are placed in an oven at 80-100° C. to dry for 6-12 hours, and then heated in a box furnace at 1000-1200° C. to sinter them, and the final material is obtained after cooling to room temperature.
[0033] a: Ordinary industrial aluminum ball b: Petrolatum temporary shell
[0034] c: Mixed ceramic powder inner shell without copper slag
[0035] d: Mixed ceramic powder shell containing copper slag e: Cavity DETAILED DESCRIPTION
[0036] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0037] Embodiment 1:
[0038] A method for preparing a core-shell structured phase change metal energy storage material comprises the following steps:
[0039] Step 1: Preparation of temporary composite core:
[0040] An industrial solid aluminum ball with a diameter of 18 mm was selected as the phase change material core, and a solid alkane mixture was used as the organic curable material. The solid alkane mixture was evenly applied on the surface of the industrial aluminum ball to a thickness of 2 mm using a spin coater to prepare a temporary composite core.
[0041] Step 2: Shell preparation:
[0042] 1) Inner shell preparation: bauxite, kyanite powder, silica powder and activated α-Al 2 O 3 The powder is used as a ceramic shell additive, the silicate adhesive is used as a binder, and the copper slag content is 0wt% to make a mixed ceramic powder inner layer material, which is evenly coated on the surface of the temporary composite core to a thickness of 1.5mm using a rotary coater.
[0043] 2) Shell preparation: The copper slag content in the mixed ceramic powder was increased to 20 wt %, and the powder was evenly coated on the surface of the single-layer shell temporary composite core to a thickness of 1.5 mm using a rotary coater to obtain a shell to make a sphere with a double-layer shell structure.
[0044] Step 3: Drying, sintering and cooling:
[0045] The prepared spheres were placed in a 75°C oven to dry for 12 hours, and then sintered in a 1100°C box furnace to obtain the final material after cooling.
[0046] When the copper slag content of the shell is 20wt%, with 300 thermal cycles as the standard, the material does not leak after 300 thermal cycle tests, proving that the stability of the material is significantly improved, and the heat storage capacity and thermal conductivity of the material are improved by 5-7%.
[0047] Embodiment 2:
[0048] A method for preparing a core-shell structured phase change metal energy storage material comprises the following steps:
[0049] Step 1: Preparation of temporary composite core:
[0050] An industrial solid aluminum ball with a diameter of 18 mm was selected as the phase change material core, and a solid alkane mixture was used as the organic curable material. The solid alkane mixture was evenly applied on the surface of the industrial aluminum ball to a thickness of 2 mm using a spin coater to prepare a temporary composite core.
[0051] Step 2: Shell preparation:
[0052] 1) Inner shell preparation: bauxite, kyanite powder, silica powder and activated α-Al 2 O 3The powder is used as a ceramic shell additive, the silicate adhesive is used as a binder, and the copper slag content is 0wt% to make a mixed ceramic powder inner layer material, which is evenly coated on the surface of the temporary composite core to a thickness of 1.5mm using a rotary coater.
[0053] 2) Shell preparation: The copper slag content in the mixed ceramic powder was increased to 10 wt %, and the copper slag was evenly coated on the surface of the single-layer shell temporary composite core to a thickness of 1.5 mm using a rotary coater to obtain a shell to make a sphere with a double-layer shell structure.
[0054] Step 3: Drying, sintering and cooling:
[0055] The prepared spheres were placed in a 75°C oven to dry for 12 hours, and then sintered in a 1100°C box furnace to obtain the final material after cooling.
[0056] When the copper slag content of the shell is 10wt%, taking 300 thermal cycles as the standard, the material leaks after 100 thermal cycle tests, and the heat storage capacity and thermal conductivity of the material are improved by 2-4%.
[0057] Embodiment 3:
[0058] A method for preparing a core-shell structured phase change metal energy storage material comprises the following steps:
[0059] Step 1: Preparation of temporary composite core:
[0060] An industrial solid aluminum ball with a diameter of 18 mm was selected as the phase change material core, and a solid alkane mixture was used as the organic curable material. The solid alkane mixture was evenly applied on the surface of the industrial aluminum ball to a thickness of 2 mm using a spin coater to prepare a temporary composite core.
[0061] Step 2: Shell preparation:
[0062] 1) Inner shell preparation: bauxite, kyanite powder, silica powder and activated α-Al 2 O 3 The powder is used as a ceramic shell additive, the silicate adhesive is used as a binder, and the copper slag content is 0wt% to make a mixed ceramic powder inner layer material, which is evenly coated on the surface of the temporary composite core to a thickness of 1.5mm using a rotary coater.
[0063] 2) Shell preparation: The copper slag content in the mixed ceramic powder was increased to 30 wt %, and the copper slag was evenly coated on the surface of the single-layer shell temporary composite core to a thickness of 1.5 mm using a rotary coater to obtain a shell to make a sphere with a double-layer shell structure.
[0064] Step 3: Drying, sintering and cooling:
[0065] The prepared spheres were placed in a 75°C oven to dry for 12 hours, and then sintered in a 1100°C box furnace to obtain the final material after cooling.
[0066] When the copper slag content of the shell is 30wt%, taking 300 thermal cycles as the standard, the material leaks after 250 thermal cycle tests, and the heat storage capacity and thermal conductivity of the material are improved by 8-9%.
[0067] Comparative Example:
[0068] A method for preparing a core-shell structured phase change metal energy storage material comprises the following steps:
[0069] Step 1: Preparation of temporary composite core:
[0070] An industrial solid aluminum ball with a diameter of 18 mm was selected as the phase change material core, and a solid alkane mixture was used as the organic curable material. The solid alkane mixture was evenly applied on the surface of the industrial aluminum ball to a thickness of 2 mm using a spin coater to prepare a temporary composite core.
[0071] Step 2: Shell preparation:
[0072] 1) Inner shell preparation: bauxite, kyanite powder, silica powder and activated α-Al 2 O 3 The powder is used as a ceramic shell additive, the silicate adhesive is used as a binder, and the copper slag content is 0wt% to make a mixed ceramic powder inner layer material, which is evenly coated on the surface of the temporary composite core to a thickness of 1.5mm using a rotary coater.
[0073] 2) Shell preparation: Apply the same inner layer material to a thickness of 1.5 mm.
[0074] Step 3: Drying, sintering and cooling:
[0075] The prepared spheres were placed in a 75°C oven to dry for 12 hours, and then sintered in a 1100°C box furnace to obtain the final material after cooling.
[0076] When the copper slag content of the outer shell is 0wt%, taking 300 thermal cycles as the standard, the material does not leak after 300 thermal cycle tests. The double-layer shell structure improves the stability of the material without adding copper slag.
[0077] It can be seen from the above embodiments and comparative examples that the double-shell energy storage material of the present invention improves the thermal conductivity and heat storage capacity of the material due to the addition of copper slag in the outer shell, but adding a suitable proportion of copper slag will also improve the stability of the material. The present invention proposes that the ideal effect is obtained when the proportion of copper slag added in the outer shell is 20wt%.
Claims
1. A copper slag core-shell structure phase change energy storage material and a preparation method thereof, characterized in that: The following steps are involved: Step 1, temporary composite core preparation The sacrificial solid alkane mixture is evenly coated on the surface of an aluminum ball of a selected diameter by a spin coater to form a shell, thereby obtaining a temporary composite core of a certain particle size as required; Step 2: Shell preparation 1) Preparation of inner shell: Use a rotary coater to evenly apply the mixed ceramic powder without copper slag on the prepared temporary composite core to obtain the inner shell. 2) Preparation of outer shell: Coat the mixed ceramic powder containing a certain proportion of copper slag on the single-layer shell to make a double-layer shell material; Step 3: Drying, sintering, cooling The prepared spheres are placed in an oven and dried at a set temperature for 6 to 12 hours, then heated in a box furnace at a set temperature and kept warm for 2 to 3 hours to sinter them, and the final material is obtained after cooling to room temperature.
2. A copper slag core-shell structure phase change energy storage material and a preparation method thereof according to claim 1, characterized in that: In the step 1, the sacrificial solid alkane mixture is petrolatum, the coating thickness is 1 to 2 mm, the rotary coater is a stainless steel cavity heating coater, the diameter of the aluminum ball is 18 to 20 mm, the Al2O3 purity is more than 90%, and the particle size range of the temporary composite core is 19 to 22 mm.
3. The phase change energy storage material with a copper slag core-shell structure and a preparation method thereof according to claim 1, characterized in that: In step 2, the ratio of the mixed ceramic powder components of the inner shell is silicate adhesive 4 ~8%;Al 2 O3 powder 4~6%; blue Crystal powder 5-8%; silicon powder 0.5-2%; bauxite 70-90%. The proportion of the mixed ceramic powder for the shell is 5-8% copper slag. 30%; Silicate adhesive 4~8%;Al 2 O 3 Powder 4-6%; Kyanite powder 6-8%; Silica powder 0.5-2%; Bauxite 65- 85%。 4. A copper slag core-shell structure phase change energy storage material and a preparation method thereof according to claim 1, characterized in that: In the step 3, the drying temperature is 80-100°C, and the sintering temperature is 1000-1200°C.