Smelting method for improving cleanliness of molten steel by combining high-MgO tundish covering agent with ladle casting operation

By using high-MgO tundra covering agent and rice husk ash in the smelting process, combined with ladle pouring operation, the problem of unstable liquid molten steel is solved, and the stable production and inclusion control of high-clean steel is achieved, ensuring that The high cleanliness and product reliability of molten steel.

CN118932133APending Publication Date: 2024-11-12CHANGZHOU ZENITH SPECIAL STEEL CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411047944.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing smelting process, liquid steel is easily contaminated by tundra covering agent during continuous casting, resulting in unstable cleanliness of the molten steel, and inclusion control is difficult to meet the requirements of high clean steel, and conventional covering agents are easily sintered or mixed with liquid steel. Reaction affects cleanliness.

Method used

High MgO tundra covering agent combined with ladle pouring operation, by discharge 3t to 4t of steel water during each furnace to remove drainage sand, and use rice husk ash as insulation covering agent to ensure that the covering agent is not sintered and does not relate to steel. Liquid reaction, maintain high cleanliness.

Benefits of technology

It effectively improves the cleanliness of the steel, ensures that the maximum inclusion size in 2000mm2 of the rolled material is ≤18μm, and the production of high-clean steel is stable, avoids pollution caused by sintering and reaction of the cover agent, and improves the stability of the steel and product reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure HDA0004974025790000011
    Figure HDA0004974025790000011
Patent Text Reader

Abstract

The invention discloses a smelting method for improving the cleanliness of molten steel through combination of a high-MgO tundish covering agent and ladle casting operation, and belongs to the technical field of clean steel production processes. The production process of the clean steel comprises the following steps: BOF-LF-RH-CCM, wherein a BOF converter is used for carrying out C and P removal treatment on molten steel; performing S removal, O removal, alloying, heating and other treatments on the molten steel by the LF refining furnace; the RH vacuum furnace is used for degassing the molten steel and removing inclusions; the CCM continuous casting machine is used for casting the molten steel, a tundish adopts a high MgO covering agent, meanwhile, 3t-4t of molten steel is firstly discharged during casting of a steel ladle of each furnace, and then the tundish is transferred back for casting. The smelting of the high-cleanliness steel is realized by combining the high-MgO tundish covering agent with the ladle casting operation. According to the invention, the detection of 2000mm < 2 > of clean rolled steel can be realized, and the size of the maximum inclusion is less than or equal to 18 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of clean steel production technology, and in particular to a smelting method for improving the cleanliness of molten steel, and in particular to a smelting method for improving the cleanliness of molten steel by utilizing a high-MgO tundish covering agent in combination with a ladle pouring operation. Background Art

[0002] The cleanliness of steel products is of great significance to ensure various properties of steel products, such as fatigue life. Among them, inclusions are typical indicators of cleanliness, and high-cleanliness steel products have clear indicators for inclusions. The typical smelting process of conventional high-cleanliness steel is BOF-LF-RH-CCM. By controlling the type of inclusions and combining the RH large cycle, a large number of inclusions in the steel can be removed, and the cleanliness of the steel after RH is greatly improved. After RH, the molten steel needs to be cast into the final ingot by CCM continuous casting. Unreasonable continuous casting process will cause secondary pollution of molten steel. Typical processes include the inflow of drainage sand when the ladle is opened, the mixed impact of steel slag when the molten steel impacts the tundish, the involvement of the tundish covering agent during continuous casting, and the rice husk ash pollution covering agent indirectly deteriorating the cleanliness of the molten steel. In order to further improve and stabilize the cleanliness of molten steel, scholars have carried out a lot of work.

[0003] The Chinese patent with publication number CN 117925948 A discloses a method for preparing ultra-pure stainless steel for automobile decorative strips, which requires that 80-100 kg of magnesium covering agent be added after the molten steel in the middle package reaches 15-20 tons, and 40-50 kg of aluminum-calcium low-melting-point covering agent be added after the molten steel in the middle package reaches 20-25 tons, wherein the composition of magnesium covering agent is MgO≥85% and Al2O3+SiO2≤10% by weight; the composition of aluminum-calcium low-melting-point covering agent is CaO≥40%, Al2O3 25-35%, and MgO+SiO2≤10%. The total oxygen content of the final continuous casting middle package sample is <20ppm, and the inclusion rating of the plate (type B+type D) is ≤1.0. The comparative patent introduces MgO covering agent (more addition) and aluminum calcium low melting point covering agent (less addition). The melting point of the final covering agent mixed by the two is between the two and is more inclined to the high melting point sintering type covering agent. This type of covering agent is prone to cracking due to sintering crusting, resulting in poor covering effect. The crusting will affect the stroke of the flow control plug rod, and finally deteriorate the cleanliness of the molten steel. On the other hand, after the aluminum calcium low melting point covering agent is added, in order to ensure the temperature of the molten steel, a layer of carbonized rice husk ash will be added to the surface of the covering agent. Its main component is SiO2. SiO2 will interact with the aluminum calcium low melting point covering agent, and the SiO2 content in the covering agent will increase. After indirectly contacting the molten steel, it will transfer the O content to the molten steel. The reaction formula (1) is [Al] 钢液 +(SiO2) 覆盖剂 →(Al2O3) 夹杂物 +[Si] 钢液, which leads to an increase in inclusions in the steel and further deteriorates the cleanliness of the molten steel.

[0004] Chinese patent CN 115673269 A reduces the melting point of the conventional tundish covering agent by adding cryolite to the covering agent, and avoids the crusting of the covering agent without adding carbonized rice husk. By using double-layer aluminum drainage sand without SiO2, Fe2O3, and Cr2O3 content, oxidizing substances are prevented from entering the tundish covering agent, and finally the number of continuous casting furnaces for bearing steel is increased from the initial 6 furnaces to more than 13 furnaces. Compared with the patent, which uses a covering agent with a lower melting point, although the covering agent can be guaranteed not to form a crust without adding carbonized rice husk, the superheat of the molten steel in the tundish needs to be greatly increased, and the segregation index of the final steel product is deteriorated; and the covering agent with a lower melting point has better wettability with the molten steel, so it is more prone to slag rolling during the continuous casting process; on the other hand, due to the introduction of aluminum drainage sand, after the drainage sand flows from the ladle into the tundish, the drainage sand and the covering agent will react, which will also cause changes in the composition of the covering agent. As the number of casting furnaces increases, the melting point will gradually increase, which will eventually affect the covering effect of the covering agent, resulting in inconsistent cleanliness of molten steel in different furnaces, and the quality of steel products cannot be guaranteed. The comparative patent selects a double-layer aluminum drainage sand that does not contain SiO2, Fe2O3, and Cr2O3. Since it does not contain oxides such as SiO2, Fe2O3, and Cr2O3, it will not react with the molten steel in the reaction formula (1) after contacting the molten steel. However, the comparative patent chooses to flow the aluminum drainage sand directly into the tundish, which causes it to directly serve as a source of aluminum inclusions in the steel, directly deteriorating the cleanliness of the molten steel.

[0005] Chinese patent CN 114799149 A provides an external ladle drainage sand device and drainage method. Taking advantage of the high temperature of molten steel and the low temperature of drainage sand, the device design includes a molten steel penetration zone and a drainage sand collection zone. The drainage sand enters the collection zone after passing through the penetration zone. When the molten steel flows to the penetration zone with the drainage sand, it breaks through the penetration zone and falls into the impact zone of the tundish. Compared with the patent, there is a large misjudgment when observing the external connection of the drainage sand by human naked eyes; and the drainage sand is mixed with the molten steel. After mixing, it enters the tundish together with the steel flow. It is impossible to judge manually with the naked eye, resulting in the possibility that the drainage sand is evacuated from the external device before being completely discharged. On the other hand, the influence of the covering agent on the molten steel is not considered. Summary of the invention

[0006] For steel products such as bearings, gears, and transmission shafts that need to withstand continuous and variable loads, it is very necessary to ensure that the inclusions in the steel products are small to ensure the longevity of the steel. The national standard GB / T 10561-2005 is too simple in its requirements for inclusion detection. It is divided into grades A, B, C, D, and DS. There are problems such as too small detection area and loose inclusion control. For high-clean steel, conventional national standard ratings can no longer meet the characterization of steel inclusion control conditions. In order to meet the requirements of efficient and reliable evaluation of whether the steel is high-clean steel, a new evaluation method has been developed based on previous customer usage and actual evaluation efficiency, that is, using rolled material to detect 2000mm 2 , the maximum inclusion size ≤18μm is used as an evaluation index, which can well distinguish the cleanliness control of steel. The maximum inclusion size ≤18μm indicates that the overall cleanliness control of the steel is good; after exceeding 18μm, the larger the value, the worse the cleanliness control ability and the lower the reliability of the steel. In view of the shortcomings of the existing methods, the purpose of the present invention is to solve the problem of stable production of high-clean steel, and finally obtain a 2000mm rolling material detection 2 , the maximum inclusion size is ≤18μm.

[0007] The technical solution adopted by the present invention is: a smelting method for improving the cleanliness of molten steel by using a high-MgO tundish covering agent combined with a ladle pouring operation, including the following requirements: The smelting method comprises the following steps: BOF converter smelting - LF refining - RH vacuum treatment - CCM continuous casting. In the CCM continuous casting step, a high-MgO covering agent and a heat-insulating covering agent are sequentially added to the tundish, and 3t~4t of molten steel are first discharged when each furnace is poured.

[0008] Furthermore, the composition requirements of high MgO quality covering agent are: MgO 95%~97%, SiO2≥3%, and inevitable impurities.

[0009] Furthermore, the high MgO covering agent is a powder with a particle size of 0.1-1.0 mm.

[0010] Furthermore, the high-MgO covering agent is added in the following manner: about 80 kg is added to the impact zone, and about 200 kg is added to the pouring zone. The adding principle is: the covering agent thickness is about 1 cm to 5 cm.

[0011] Furthermore, the heat-insulating covering agent is rice husk ash, which is a covering agent with excellent heat-insulating effect and can be added at any time as needed.

[0012] Specifically, the smelting method for improving the cleanliness of molten steel by using a high-MgO tundish covering agent combined with a ladle pouring operation comprises the following steps: (1) Converter smelting: conventional smelting; Furthermore, the end point temperature of BOF converter smelting is ≥1580°C, the end point C is ≥0.05%, and the end point P is ≤0.035%; aluminum blocks, alloys and slag are added after steelmaking.

[0013] (2) LF refining: conventional smelting after arrival; Furthermore, the LF tapping temperature is ≥1580°C to complete alloying.

[0014] (3) RH vacuum treatment: conventional smelting; Furthermore, the RH vacuum treatment time is ≥15min; the soft blowing time is ≥5min.

[0015] (4) In CCM continuous casting, high MgO covering agent and rice husk ash are added to the tundish, and 3t~4t of molten steel must be discharged before pouring each furnace.

[0016] The requirement of MgO: 95%~97% for high MgO quality covering agent is as follows: First, MgO is selected as covering agent because its melting point is 2800℃. Usually, when a single powder is heated to a temperature of about 2 / 3 of its melting point, sintering will occur. During continuous casting, the temperature of molten steel is about 1500℃~1550℃. Since MgO has a very high melting point, it will not sinter (2 / 3 of the melting point of MgO is 1867℃, and the temperature of the continuous casting molten steel has not reached the sintering temperature). It will remain in powder form and cover the surface of the molten steel during the casting process. The melting points of Al2O3 and MgO·Al2O3 are 2054ºC and 2105℃, respectively. The 2 / 3 melting point temperature is about 1400℃, and the temperature of the continuous casting molten steel meets the sintering conditions. Therefore, sintering problems are very likely to occur during molten steel casting. Once the covering layer is sintered, a series of defects such as crusting and cracking will occur. Oxygen or the upper layer of rice husk ash will contact the molten steel, affecting the cleanliness of the molten steel. On the other hand, since MgO has a high melting point and does not sinter and always maintains a dense powder state, it will not react with MgO powder after being covered with a layer of rice husk ash with a better heat preservation effect. Therefore, it will not affect the composition of the MgO covering agent during the continuous casting process, and SiO2 will not contact the molten steel, causing indirect oxygen transfer problems. Finally, the wettability of molten steel and solid powdered MgO particles is poor, and the interaction between the two is extremely weak, which will not affect the composition of the molten steel. In addition, the probability of the covering agent being involved is greatly reduced due to the lack of wetting, and it will not cause the impact of the entanglement type hazard. Secondly, if the MgO content is less than 95%, there will be more impurities, which will affect the composition of the covering agent and cause it to sinter or react with rice husk ash, which is not conducive to the control of the cleanliness of the molten steel; if the MgO content is greater than 97%, the manufacturing cost of purification is too high, which is not conducive to production economy. Therefore, the most suitable MgO content is 95%~97%.

[0017] The reason why 3t~4t of molten steel must be discharged before pouring each furnace is that the components of conventional drainage sand are mainly SiO2, Fex O, Cr2O3, which are poured into the bottom of the downspout position of the ladle before the ladle receives the molten steel. When the ladle is lifted to the tundish and the long nozzle is opened, they are broken by the static pressure of the molten steel and flow out with the steel flow. Since the main component of the drainage sand is weak oxide, it will react with the molten steel in a similar manner to reaction formula (1). Therefore, it must be strictly prevented from entering the molten steel for high-clean steel smelting. In addition, in the present invention, once the drainage sand flows into the tundish and reacts with the MgO-based covering agent, it will also deteriorate the performance of the covering agent and cannot play the role of the MgO-based covering agent. In order to prevent the drainage sand from flowing into the tundish, the conventional operation method is to manually hold a sand receiving device to catch part of the drainage sand at the moment when the steel flows down. This method relies entirely on manual judgment. In actual production, a lot of drainage sand has entered the tundish with the steel flow and finally deteriorated the cleanliness of the molten steel. For each furnace, 3t~4t of molten steel must be discharged first when pouring. The purpose is to completely discharge the drainage sand and ensure that the casted molten steel is molten steel without drainage sand components. If the weight of molten steel discharged during pouring is less than 3t, the drainage sand will still not be completely discharged; if the weight of molten steel discharged during pouring is greater than 4t, the discharge volume will be too large and the cost will increase. Therefore, the most reasonable weight of molten steel discharged during pouring is 3t~4t. The discharged molten steel can be added back to the refining furnace for re-smelting.

[0018] The beneficial effects of the present invention are: the use of high MgO covering agent, combined with the discharge of 3t~4t of molten steel during pouring, improves the cleanliness of molten steel and ensures the inspection of rolled materials at 2000mm 2 , the maximum inclusion size is ≤18μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of the implementation process of the present invention: Figure 1 (a) is a side view of the casting process. Figure 1 (b) is a top view, where the ladle outlet is rotated to the overflow trough to discharge molten steel before pouring. Figure 1 (c) is a top view, showing normal casting after the steel flow is discharged before pouring; Figure 2 Example 1: The largest inclusion morphology (13.06 μm); Figure 3 Example 2: The largest inclusion morphology (17.27 μm); Figure 4 Comparative Example 1: Maximum inclusion morphology (27.25 μm); Figure 5 Comparative Example 2: Maximum inclusion morphology (39.67 μm); Figure 6 Comparative Example 3: Maximum inclusion morphology (22.05 μm); Figure 7Comparative Example 4: Maximum inclusion morphology (34.71 μm); Figure 8 The morphology of the largest inclusion in comparative example 5 (13.86 μm); Fig. 9 Morphology of the largest inclusion in Comparative Example 6 (28.88 μm). DETAILED DESCRIPTION

[0020] The present invention is further described below in conjunction with the accompanying drawings and embodiments. This figure is a simplified schematic diagram, which only illustrates the basic structure of the present invention in a schematic manner, and therefore it only shows the components related to the present invention.

[0021] Taking 20Cr for automobile gears as an example, the production of high-clean steel is organized. The standard composition requirements of the steel grade are shown in Table 1.

[0022] Table 1 Standard composition of 20Cr steel, %

[0023] The main production processes of each process are as follows: BOF: Add about 10t of pig iron, about 30t of scrap steel, about 120t of molten iron, oxygen supply time about 15min, oxygen pressure 0.9MPa, oxygen consumption about 8000m 3 , add about 4000kg of lime, about 1300kg of light-burned dolomite, about 600kg of raw dolomite, about 1500kg of ore, the end point of steelmaking C is about 0.065%, P is about 0.018%, S is about 0.03%, the tapping temperature is about 1615℃, about 800kg of silicon manganese, about 380kg of ferrosilicon, about 1700kg of low-carbon ferrochrome, about 130kg of aluminum block, about 200kg of refined slag, and about 400kg of lime.

[0024] LF: The ladle temperature is about 1530℃, the power supply time is about 35min, the smelting time is about 60min, and about 20kg of fluorite, about 200kg of lime, about 50kg of aluminum particles, about 220kg of silicon carbide, about 180kg of silicon manganese, about 80kg of ferrosilicon, about 400kg of high carbon ferrochrome, about 50kg of carburizer are added during the smelting process for alloying, and the LF ladle temperature is about 1600℃. The composition of the molten steel is roughly controlled as follows: C: 0.20%, Si: 0.22%, Mn: 0.60%, P: 0.01%, S: 0.007%, Al: 0.025%, Cr: 0.80%.

[0025] RH: inlet temperature is about 1597℃, RH end temperature is about 1570℃, degassing time is about 20min, pressure holding time is about 15min, ultimate vacuum degree ≤67Pa, gas flow rate is 100Nm 3 / h, lifting gas type Ar, no calcium wire feeding after breaking air. Soft blowing time is about 25min, and the bag temperature is about 1560℃. The composition of molten steel is roughly controlled as follows: C: 0.20%, Si: 0.22%, Mn: 0.60%, P: 0.01%, S: 0.0068%, Al: 0.023%, Cr: 0.80%.

[0026] CCM: The conventional continuous casting superheat is about 30°C, the crystallizer water flow rate is about 2000L / min, the specific water volume is 0.3L / kg, the crystallizer electromagnetic stirring current is 230A, the end electromagnetic stirring current is 180A, the casting speed is 1m / min, and the integral internal water inlet and stopper rod are used for flow control.

[0027] Covering agent types are divided into ① Type A covering agent, composition: MgO: 96%~97%, SiO2: 3%~4%, and the rest are unavoidable impurities; ② Type B covering agent, composition: MgO: 95%~96%, SiO2: 4%~5%, and the rest are unavoidable impurities; ③ Type C covering agent, composition: MgO: 90%~91%, SiO2: 9%~10%, and the rest are unavoidable impurities; ④D-type covering agent, components: CaO: 38%, Al2O3: 32%, CaF2: 10%, MgO: 6%, SiO2: 2%, and the rest are unavoidable impurities (melting point < 1500℃).

[0028] The operation areas during pouring are divided into: ① Operation I: Before pouring, rotate the ladle outlet to the overflow trough, discharge 3.5t of molten steel, and then return to the casting position to start pouring again for conventional casting; ② Operation II: Before pouring, rotate the ladle outlet to the overflow trough, discharge 3 tons of molten steel, and then return to the casting position to start pouring again for conventional casting; ③ Operation III: Manually use the sand receiving device to receive the flowing sand when pouring, and continue the normal casting after completing the sand receiving action; ④Operation IV: Directly discharge the drainage sand into the tundish and perform conventional casting.

[0029] The addition of rice husk ash is divided into: ①Add as needed at any time and place on the covering agent; ②No addition.

[0030] Statistics: (1) Select the corresponding furnace ingots and transfer them to the rolling mill for rolling with the same process. All are rolled into φ55mm bars. Samples are taken at 1 / 2 radius of the rolled material. 20 samples are cut longitudinally, and the area of ​​each sample is 100mm. 2 , and the final maximum inclusion size was recorded using an optical microscope.

[0031] (2) Five ingots were selected for low-magnification central carbon segregation analysis, and the average value was used to characterize the carbon segregation (the closer to 1, the more uniform). Example 1

[0032] The covering agent used is type A covering agent: composition MgO: 96.37%, SiO2: 3.28%. Operation I of pouring: before pouring, rotate the ladle outlet to the overflow tank, discharge 3.5t of molten steel, and then return to the casting position to start pouring again for normal casting. Rice husk ash can be added as needed and placed on the covering agent.

[0033] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 2 shown. Example 2

[0034] The covering agent used is type B covering agent, with the composition of MgO: 95.21%, SiO2: 4.36%. Operation II is performed before pouring: before pouring, the ladle outlet is rotated to the overflow tank, and after 3 tons of molten steel is discharged, it is restored to the casting position and poured again for normal casting. Rice husk ash is added as needed and placed on the covering agent.

[0035] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 3 shown. Comparative Example 1

[0036] The covering agent used is type C covering agent, with the composition of MgO: 90.29%, SiO2: 9.08%. Operation I of pouring: Before pouring, rotate the ladle outlet to the overflow tank, discharge 3.5t of molten steel, and then return to the casting position to start pouring again for normal casting. Rice husk ash can be added as needed and placed on the covering agent.

[0037] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 4 shown. Comparative Example 2

[0038] The D-type covering agent is used, with the composition of CaO: 38.21%, Al2O3: 32.31%, CaF2: 10.84%, MgO: 6.54%, SiO2: 2.61%. Operation I of pouring: Before pouring, rotate the ladle outlet to the overflow tank, discharge 3.5t of molten steel, and then return to the casting position to start pouring again for normal casting. Rice husk ash can be added as needed and placed on the covering agent.

[0039] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 5 shown. Comparative Example 3

[0040] The covering agent used is type A covering agent, with the composition of MgO: 96.64%, SiO2: 3.29%. Operation III is performed when pouring: the sand receiving device is used to manually receive the flowing sand during pouring, and the normal casting is continued after the sand receiving action is completed. Rice husk ash can be added at any time as needed and placed on the covering agent.

[0041] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 6 shown. Comparative Example 4

[0042] The covering agent used is type A covering agent, with the composition of MgO: 96.64%, SiO2: 3.25%. Operation IV is performed after pouring: the drainage sand is directly discharged into the tundish, and then the conventional casting is performed. Rice husk ash is added as needed at any time and placed on the covering agent.

[0043] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 7 shown. Comparative Example 5

[0044] The covering agent used is type A covering agent: composition MgO: 96.59%, SiO2: 3.28%. Operation I of pouring: before pouring, rotate the ladle outlet to the overflow tank, discharge 3.5t of molten steel, and then return to the casting position to start pouring again for normal casting. No rice husk ash is added (the superheat of the middle ladle is deliberately controlled to 80℃).

[0045] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Figure 8 shown. Comparative Example 6

[0046] The D-type covering agent is used: the composition is CaO: 38.71%, Al2O3: 32.78%, CaF2: 10.51%, MgO: 6.21%, SiO2: 2.19%. Operation I of pouring: before pouring, rotate the ladle outlet to the overflow tank, discharge 3.5t of molten steel, and then return to the casting position to start pouring again for normal casting. No rice husk ash is added (the superheat of the middle ladle is deliberately controlled to 80℃).

[0047] Track the results of the rolled material inclusion detection, where the maximum inclusion size is shown in Fig. 9 shown.

[0048] The inclusion and segregation data of the embodiments and comparative examples are shown in Table 1 below.

[0049] Table 1 Inclusion comparison table

[0050]

[0051] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A smelting method for improving the cleanliness of molten steel by using a high-MgO tundish covering agent combined with ladle pouring operation, It is characterized in that The smelting method comprises the following steps: BOF converter smelting - LF refining - RH vacuum treatment - CCM continuous casting; in the CCM continuous casting step, a high-MgO covering agent and a heat-insulating covering agent are sequentially added to the tundish, and 3t~4t of molten steel is first discharged when each furnace is poured.

2. The smelting method of improving the cleanliness of molten steel by using a high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that The composition requirements of the high MgO covering agent are: MgO 95%~97%, SiO 2 ≥3%, and unavoidable impurities.

3. The smelting method of improving the cleanliness of molten steel by using a high-MgO tundish covering agent combined with ladle pouring operation according to claim 2, It is characterized in that The high MgO covering agent is a powder with a particle size of 0.1~1.0mm.

4. The smelting method of improving the cleanliness of molten steel by using a high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that The principle of adding the high MgO covering agent is: the thickness of the covering agent is 1cm~5cm.

5. The smelting method of improving the cleanliness of molten steel by using high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that The thermal insulation covering agent is rice husk ash.

6. The smelting method of improving the cleanliness of molten steel by using high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that The BOF converter smelting has an end point temperature of ≥1580°C, an end point C of ≥0.05%, and an end point P of ≤0.035%; and aluminum blocks, alloys and slag are added after steel is tapped.

7. The smelting method of improving the cleanliness of molten steel by using high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that In the LF refining, the tapping temperature is ≥1580°C to complete the alloying.

8. The smelting method of improving the cleanliness of molten steel by using high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that The RH vacuum treatment time is ≥15min; the soft blowing time is ≥5min.

9. The smelting method of improving the cleanliness of molten steel by using high-MgO tundish covering agent combined with ladle pouring operation according to claim 1, It is characterized in that The index of the high clean steel obtained by the smelting method is to detect the rolled material at 2000mm 2 , the maximum inclusion size is ≤18μm.

Citation Information

Patent Citations

  • External steel ladle filler sand device and drainage method

    CN114799149A

  • Continuous casting method for stably controlling components of bearing steel tundish covering agent

    CN115673269A

  • Preparation method of ultra-pure stainless steel for automobile decoration strip

    CN117925948A