Steering shaft production process
Through the process flow of spheroidized annealing, phosphating and saponification, the hardness control and friction problems in the cold heading of the steering shaft are solved, and the quality and pass rate of the product are improved.
Patent Information
- Application Number
- CN202410990320.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing steering shaft cold heading process, the hardness of steel is difficult to control, resulting in deformation and crack problems, and the friction during the cold heading process is large, affecting product quality.
The process flow of spheroidization annealing, phosphating treatment and saponification treatment is adopted. After the drawing treatment, spheroidization annealing, phosphating liquid and saponification liquid are treated, the lubricating film is formed, the hardness and friction during the cold heading process is controlled, and the product quality is improved.
It effectively improves the cold heading quality of the steering shaft, avoids deformation and cracks, reduces friction, and improves the product's pass rate and contour accuracy.
Smart Images

Figure BDA0004958685880000091 
Figure BDA0004958685880000101 
Figure BDA0004958685880000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steering shaft processing, in particular to a steering shaft production process. Background Art
[0002] The steering shaft is the shaft in the steering column of the car that is connected to the steering wheel. It is used to transmit the rotation of the steering wheel to the steering gear. The steering shaft is one of the important parts of the car. Its processing accuracy is very high. How to ensure the accuracy of the workpiece in the processing technology is the key to achieving safe and qualified products.
[0003] Most steering shafts are produced by cold heading process. Before the cold heading process, the steel billet needs to be spheroidized annealed and phosphate saponified. After the existing medium carbon steel is spheroidized, the hardness is basically controlled between 75-79HRB. When the hardness exceeds 79HRB, the steel is severely decarburized, and tertiary cementite will precipitate along the grain boundary, which will deteriorate the cold heading performance of the steel and cause cold heading cracking. In addition, due to the small diameter of the steering shaft, it is easy to deform during the cold heading process, resulting in the profile of the steering shaft not meeting the requirements. Moreover, when the cold heading plasticity of the steel is not enough, that is, the deformation degree required by the cold heading product exceeds the limit deformation degree of the steel, it will cause cracks on the surface of the cold heading workpiece. Summary of the invention
[0004] In order to improve the qualified rate of steering shaft during cold heading, the present invention provides a steering shaft production process.
[0005] The present invention provides a steering shaft production process that adopts the following technical solution: A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 750-770°C, kept warm for 30-90 minutes, cooled to 690-710°C with the furnace and kept warm for 3-5 hours, then cooled to 490-520°C with the furnace and then air-cooled; S3 phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50-70 ℃ and kept at a constant temperature for 15-25 minutes and then air-dried; S4. Saponification treatment, the phosphating steel billet is placed in a saponification solution at a constant temperature of 55-65 ° C for 4-8 minutes and then dried; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0006] Preferably, in step S2, the cooling rate during furnace cooling to 690-710°C is 12-17°C / hour.
[0007] Preferably, in step S2, the cooling rate during furnace cooling to 690-710°C is 14-15°C / hour.
[0008] Preferably, the phosphating solution comprises 40-50 parts of phosphoric acid, 20-30 parts of citric acid, 5-12 parts of nitrate, 5-10 parts of zinc dihydrogen phosphate, and 3-7 parts of surfactant in parts by weight.
[0009] Preferably, the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:(1-3).
[0010] Preferably, the surfactant includes one or both of sodium fatty alcohol polyoxyethylene ether sulfate and sodium dodecyl sulfate.
[0011] Preferably, the weight ratio of the sodium fatty alcohol polyoxyethylene ether sulfate to sodium dodecyl sulfate is 1:1.
[0012] Preferably, the saponification solution comprises 20-25 parts of stearic acid, 1.5-3.5 parts of sodium hydroxide, 6-7 parts of triethanolamine, and 390-400 parts of water in a weight ratio.
[0013] Preferably, the saponification solution also includes 1-4 parts of sodium nitrite.
[0014] Preferably, the drying temperature in step S4 is 140-180°C.
[0015] In summary, the present invention has the following beneficial effects: 1. After the steel billet is subjected to the spheroidizing annealing treatment of the present application, the hardness of the steel billet can be improved, and deformation of the steel billet during the cold heading process can be avoided. After the steel billet after the spheroidizing annealing treatment is treated with phosphating liquid and saponifying liquid, a lubricating film is formed on the surface of the steel billet, which prevents the surface of the steel billet from being scratched during the cold heading process, thereby improving the quality of the cold heading of the steel billet.
[0016] 2. In the present application, the cooling rate is limited to 12-17°C / hour, especially 14-15°C / hour, which can effectively avoid the precipitation of lamellar cementite and effectively reduce the embrittlement of the steel billet during cold heading.
[0017] 3. In the phosphating solution of the present application, the combined use of phosphoric acid and citric acid can promote the corrosion effect of phosphoric acid on the surface of the steel billet, so that manganese nitrate and zinc dihydrogen phosphate can form a phosphating film on the surface of the steel billet. At the same time, citric acid can improve the stability of the phosphating effect and improve the crystallization state of the phosphating film. The addition of nickel nitrate can promote the film formation rate of manganese nitrate and zinc dihydrogen phosphate on the surface of the steel billet. At the same time, nickel nitrate can eliminate surface polarization and improve the quality of the phosphating film.
[0018] 4. The combination of the saponification liquid, saponification temperature and time in the present application can make the thickness of the saponification film formed on the surface of the steel billet relatively uniform, with good lubrication effect, which can effectively reduce the friction coefficient during the cold heading process and improve the processing quality of the cold heading process. When the saponification time is relatively long, the saponification film on the surface of the steel billet is relatively thick, and the saponification film is easy to fall off during cold heading. When the saponification time is relatively short, the saponification film is too thin and the lubrication effect cannot be achieved. DETAILED DESCRIPTION
[0019] The present invention is further described in detail below with reference to the embodiments.
[0020] The raw materials used in the examples and comparative examples of the present application are all commercially available.
[0021] In the examples and comparative examples of the present application, the steel billets are made of No. 45 steel.
[0022] Sodium fatty alcohol polyoxyethylene ether sulfate, CAS number is 68585-34-2.
[0023] Example 1 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 750°C, kept warm for 30 minutes, cooled to 690°C with a cooling rate of 12°C / hour, kept warm for 5 hours, and then cooled to 490°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0024] Example 2 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 12°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0025] Example 3 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 770°C, kept warm for 90 minutes, cooled to 710°C with a cooling rate of 12°C / hour, kept warm for 3 hours, and then cooled to 520°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0026] Example 4 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 14°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0027] Example 5 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 15°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0028] Example 6 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 17°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0029] Example 7 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 10°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0030] Example 8 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 20°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50°C and kept at a constant temperature for 15 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 55 ° C and kept at a constant temperature for 4 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0031] Example 9 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 15°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 60°C and kept at a constant temperature for 20 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 60 ° C and kept at a constant temperature for 6 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0032] Example 10 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 15°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 70°C and kept at a constant temperature for 25 minutes and then air-dried; the phosphating solution comprises 40kg of phosphoric acid, 20kg of citric acid, 5kg of nitrate, 5kg of zinc dihydrogen phosphate, and 3kg of sodium sulfate of fatty alcohol polyoxyethylene ether, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 2.5kg of manganese nitrate and 2.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 65 ° C and kept at a constant temperature for 8 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0033] Embodiment 11 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 15°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 60°C and kept at a constant temperature for 20 minutes and then air-dried; the phosphating solution comprises 45kg of phosphoric acid, 25kg of citric acid, 9kg of nitrate, 8kg of zinc dihydrogen phosphate, and 5kg of sodium dodecyl sulfate by weight, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 4.5kg of manganese nitrate and 4.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 60 ° C and kept at a constant temperature for 6 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0034] Example 12 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 15°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 60°C and kept at a constant temperature for 20 minutes and then air-dried; the phosphating solution comprises 50kg of phosphoric acid, 30kg of citric acid, 12kg of nitrate, 10kg of zinc dihydrogen phosphate, and 7kg of sodium dodecyl sulfate by weight, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 6kg of manganese nitrate and 6kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 60 ° C and kept at a constant temperature for 6 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 20kg, sodium hydroxide 1.5kg, triethanolamine 6kg, water 390kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0035] Embodiment 13 A steering shaft production process includes the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 760°C, kept warm for 60 minutes, cooled to 700°C with a cooling rate of 15°C / hour, kept warm for 3 hours, and then cooled to 500°C with the furnace and then air-cooled; S3. Phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 60°C and kept at a constant temperature for 20 minutes and then air-dried; the phosphating solution comprises 45kg of phosphoric acid, 25kg of citric acid, 9kg of nitrate, 8kg of zinc dihydrogen phosphate, and 5kg of sodium dodecyl sulfate by weight, wherein the nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:1, i.e., 4.5kg of manganese nitrate and 4.5kg of nickel nitrate; S4 saponification treatment, the phosphating steel billet was placed in a saponification solution at 60 ° C and kept at a constant temperature for 6 minutes and then dried at a temperature of 140 ° C; the saponification solution comprises a weight ratio of stearic acid 25kg, sodium hydroxide 3.5kg, triethanolamine 7kg, water 400kg; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
[0036] Embodiment 14 A steering shaft production process, which is different from Example 11 in that the nitrate includes manganese nitrate and nickel nitrate in a weight ratio of 1:2, that is, manganese nitrate is 3kg and nickel nitrate is 6kg, and the rest is the same as Example 11.
[0037] Embodiment 15 A steering shaft production process, which is different from Example 11 in that the nitrate includes manganese nitrate and nickel nitrate in a weight ratio of 1:3, that is, manganese nitrate is 2.25 kg and nickel nitrate is 6.75 kg, and the rest is the same as Example 11.
[0038] Example 16 A steering shaft production process, which is different from Example 11 in that the nitrate is 9 kg of manganese nitrate, and the rest is the same as Example 11.
[0039] Embodiment 17 A steering shaft production process, which is different from Example 11 in that the nitrate is 9 kg of nickel nitrate, and the rest is the same as Example 11.
[0040] Embodiment 18 A steering shaft production process, which is different from Example 11 in that the saponification liquid also includes 1 kg of sodium nitrite, and the rest is the same as Example 11.
[0041] Embodiment 19 A steering shaft production process, which is different from Example 11 in that the saponification liquid also includes 4 kg of sodium nitrite, and the rest is the same as Example 11.
[0042] Embodiment 20 A steering shaft production process, which is different from Example 11 in that the surfactant in the phosphating solution is composed of fatty alcohol polyoxyethylene ether sodium sulfate and sodium dodecyl sulfate in a weight ratio of 1:1, that is, the fatty alcohol polyoxyethylene ether sodium sulfate is 2.5 kg and the sodium dodecyl sulfate is 2.5 kg, and the rest is the same as Example 11.
[0043] Comparative Example 1 A steering shaft production process, which is different from Example 1 in that the temperature in the annealing furnace in step S2 is 780°C. After being kept warm for 30 minutes, it is cooled to 715°C with the furnace at a cooling rate of 12°C / hour and kept warm for 5 hours. It is then cooled to 490°C with the furnace and air-cooled. The rest is the same as Example 1.
[0044] Comparative Example 2 A steering shaft production process, which is different from Example 1 in that the temperature in the annealing furnace in step S2 is 740°C, and after being kept warm for 30 minutes, it is cooled to 680°C with the furnace at a cooling rate of 12°C / hour and kept warm for 5 hours, and then cooled to 490°C with the furnace and air-cooled. The rest is the same as Example 1.
[0045] Performance Testing The Rockwell hardness of the steel billets obtained in step S2 of the above embodiment and comparative example was measured, and the adhesion of the saponification film of the steel billets after saponification was tested. The adhesion was tested by the cross-hatch method, where grade 0 was the best and grade 5 was the worst. The steering shaft obtained by cold heading was tested for appearance integrity and the profile error of the steering shaft was measured. The test results are shown in Table 1.
[0046] Table 1 Test results of examples and comparative examples From Table 1 we can see that: The hardness of the steel billets obtained after spheroidizing annealing in Examples 1-3 of the present application is above 85HRB, and the profile error of the steering shaft finally obtained is small. Although there are cracks on the surface of the phosphorus saponification film on the surface of the steering shaft, there are no metal bright spots.
[0047] Compared with Example 2, when the cooling rate gradually increases, the hardness of the steel billet obtained in Example 4-6 shows a trend of first increasing and then decreasing. It can be seen that the cooling rate of the present application is more conducive to the steel billet having good hardness.
[0048] Compared with Example 2, when the cooling rate is not within the range specified in the present application, the hardness of the steel billet obtained in Examples 7 and 8 is lower than that in Example 2, and the profile error of the steering shaft obtained at last is also increased. This can further illustrate that when the cooling rate is limited within the range of the present application, the hardness of the steel billet can be guaranteed while the profile error of the steering shaft can be reduced.
[0049] Compared with Example 9, when the ratio of each component in the phosphating solution and the saponifying solution is changed, the adhesion of the saponified film obtained in Examples 11-13 is improved compared with that in Example 9, and after cold heading treatment, the appearance of the film is uniform and complete, and no cracks appear. It can be seen that the combination of the phosphating solution and the saponifying solution in the examples of the present application can help ensure the quality of cold heading.
[0050] Compared with Example 11, when only manganese nitrate or nickel nitrate is used as the nitrate in Examples 16-17, cracks appear on the surface of the steering shaft film obtained at last. It can be seen that the combined use of nickel nitrate and manganese nitrate can help ensure the integrity of the film surface.
[0051] Compared with Example 1, when the temperature of the spheroidizing degradation treatment is not within the range specified in the present application, the hardness of the steel billets obtained in Comparative Examples 1-2 is lower than the hardness of the steel billets obtained in Example 1. It can be seen that when the temperature of the spheroidizing annealing in the present application is limited within the range of the present application, the hardness of the steel billets can be effectively guaranteed.
[0052] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A steering shaft production process, It is characterized in that The method comprises the following preparation steps: S1. Drawing the steel billet; S2. Spheroidizing annealing, the steel billet obtained in step S1 is sent to an annealing furnace and heated to 750-770°C, kept warm for 30-90 minutes, cooled to 690-710°C with the furnace and kept warm for 3-5 hours, then cooled to 490-520°C with the furnace and then air-cooled; S3 phosphating treatment, the steel billet obtained in step S2 is placed in a phosphating solution at a temperature of 50-70 ℃ and kept at a constant temperature for 15-25 minutes and then air-dried; S4. Saponification treatment, the phosphating steel billet is placed in a saponification solution at a constant temperature of 55-65 ° C for 4-8 minutes and then dried; S5. The steel billet obtained by saponification treatment is subjected to cold heading treatment.
2. A steering shaft production process according to claim 1, Features: In the step S2, the cooling rate of the furnace cooling to 690-710°C is 12-17°C / hour.
3. A steering shaft production process according to claim 1, Features: In the step S2, the cooling rate of the furnace cooling to 690-710°C is 14-15°C / hour.
4. A steering shaft production process according to claim 1, Features: The phosphating solution comprises 40-50 parts of phosphoric acid, 20-30 parts of citric acid, 5-12 parts of nitrate, 5-10 parts of zinc dihydrogen phosphate and 3-7 parts of surfactant by weight.
5. A steering shaft production process according to claim 4, Features: The nitrate comprises manganese nitrate and nickel nitrate in a weight ratio of 1:(1-3).
6. A steering shaft production process according to claim 4, Features: The surfactant includes one or both of sodium fatty alcohol polyoxyethylene ether sulfate and sodium dodecyl sulfate.
7. A steering shaft production process according to claim 6, Features: The weight ratio of the sodium fatty alcohol polyoxyethylene ether sulfate to sodium lauryl sulfate is 1:
1.
8. A steering shaft production process according to claim 1, Features: The saponification liquid comprises 20-25 parts of stearic acid, 1.5-3.5 parts of sodium hydroxide, 6-7 parts of triethanolamine and 390-400 parts of water in a weight ratio.
9. A steering shaft production process according to claim 8, Features: The saponified solution also includes 1-4 parts of sodium nitrite.
10. A steering shaft production process according to claim 1, Features: The drying temperature in step S4 is 140-180°C.