Method for separating rhenium and molybdenum by using quaternary phosphonium salt modified material

The quaternary scale salt modified material selective adsorption and elution of rhenium in the molybdenum ore leaching solution is solved, and the problem of low separation efficiency between rhenium and molybdenum in the prior art is achieved, efficient and economical rhenium recovery and material regeneration are achieved. Suitable for industrial-scale applications.

CN118932196APending Publication Date: 2024-11-12WUHAN POLYTECHNIC UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411030301.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art method of separating rhenium and molybdenum in molybdenum ore is inefficient, and the adsorbent is costly and has poor reusability, making it difficult to apply on a large scale in the industry.

Method used

The rhenium in the molybdenum ore leaching solution was selectively adsorbed and recovered by quaternary scale salt modification material. The material was adsorbed by adjusting the solution pH value, and elution was used to achieve rhenium recovery and material regeneration.

Benefits of technology

It achieves efficient and economical rhenium recycling, overcomes the problems of high cost and poor reusability of adsorbents, is suitable for industrial-scale rhenium recycling, and the materials can be reused.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932196A_ABST
    Figure CN118932196A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of resource utilization and environmental protection, and discloses a method for separating rhenium and molybdenum by using a quaternary phosphonium salt modified material. The method comprises the following steps: 1) adding a quaternary phosphonium salt modified material into a solution containing rhenium and molybdenum, or injecting the solution into the quaternary phosphonium salt modified material, and adjusting the pH value of the solution, so that the quaternary phosphonium salt modified material selectively adsorbs rhenium; and 2) after adsorption, eluting the rhenium loaded on the material by using an eluent, concentrating and separating to realize recovery of the rhenium and regeneration of the material at the same time. By adjusting the pH value of the liquid to be adsorbed, rhenium and molybdenum can be effectively separated by using the quaternary phosphonium salt modified material, the rhenium is selectively captured, the loaded rhenium can be eluted by using the eluent, and the elution efficiency is high; after elution, the modified material is regenerated and can be repeatedly used. The technical problems of high adsorbent cost, poor reusability, complex synthesis of most nano materials, low adsorption capacity, poor selectivity and the like in the existing rhenium-molybdenum separation process are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resource utilization and environmental protection, and specifically is a method for separating rhenium and molybdenum by using quaternary phosphorus salt modified materials. Background Art

[0002] Rhenium (Re) is one of the rarest metals in the earth's crust. Due to its high melting point, high hardness, corrosion resistance and excellent mechanical properties, it is widely used as a heat-resistant material in the aviation / aerospace field and as a refining catalyst in petrochemical products. However, rhenium is usually associated with minerals such as molybdenite and copper sulfide. If the associated rhenium can be recovered during molybdenum mining, it will not only improve the economic benefits of ore mining, but also meet the growing demand for rhenium. The key to extracting associated rhenium from molybdenum ore is to selectively separate rhenium from these ore leachates. Therefore, the development of adsorbents that can selectively adsorb and separate rhenium from molybdenum ore leachates has important research value and broad application prospects.

[0003] At present, the methods for rhenium separation include chemical precipitation, ion exchange, membrane filtration, adsorption, etc. Among these common technologies, adsorption technology has the characteristics of simple operation, technical economy and low cost. In particular, adsorption technology is suitable for the treatment of low concentrations of metal ions. The most critical part of the adsorption method is the adsorbent. The adsorbents for recovering rhenium mainly include nanomaterials (nanosilica), biomass carbon, mesoporous materials, hydrogels, chitosan, etc. However, these adsorbents have challenges such as high cost, poor reusability, complex synthesis of most nanomaterials, low adsorption capacity, and poor selectivity. In addition, nanomaterial adsorbents are difficult to fill and use in adsorption columns and cannot be used in industrial separations.

[0004] Phosphonium-based ionic liquids are a class of ionic liquids containing quaternary phosphonium cations. These compounds usually form cations with four alkyl or aryl groups combined with a phosphorus atom, and are paired with various anions to form ionic liquids. Quaternary phosphonium ionic liquids are widely used in catalysis, separation, materials science, electrochemistry and other fields due to their high selectivity, low volatility, high thermal stability, adjustability, green environmental protection characteristics, and easy recovery and reuse. Studies have found that quaternary phosphonium ionic liquids can efficiently extract rhenium. However, in the extraction process, there are problems such as large amount of ionic liquid, difficult recovery, and high cost. In order to avoid the shortcomings of quaternary phosphonium ionic liquids when used directly as extractants, some people immobilize ionic liquids on substrates. For example, CN117797761A discloses a quaternary carbon nanotube material with good ReO4-adsorption and separation performance. Although rhenium can be adsorbed by immobilizing quaternary phosphonium ionic liquids onto substrates, molybdenite contains metallic molybdenum, which has similar chemical properties and atomic radius to rhenium, and rhenium only contains 200 to 800 ppm in molybdenite. Therefore, it is very difficult to recover and separate low concentrations (10 to 100 ppm) of rhenium from complexes containing coexisting metal ions, especially when molybdenum is also contained therein. There is currently no report that quaternary phosphonium adsorbents can separate rhenium and molybdenum.

[0005] In order to cope with the high demand for rhenium in industrial production and reduce the environmental pollution caused by rhenium, it is particularly important to develop a new type of efficient, economical and environmentally friendly rhenium recovery material. Summary of the invention

[0006] In view of the above defects or improvement needs of the prior art, the present invention provides a method for separating rhenium and molybdenum using a quaternary phosphonium salt modified material, and uses the quaternary phosphonium salt modified material to separate and recover rhenium in the molybdenum ore leachate, thereby solving the technical problems of low separation efficiency and inability to be applied on a large scale in the prior art separation and enrichment methods of rhenium. The quaternary phosphonium salt modified material overcomes the various limitations of existing adsorbents, and should not only have high adsorption capacity, good selectivity and reusability, but also be easy to apply industrially, and effectively meet the dual needs of efficient recovery of rhenium resources and environmental protection.

[0007] The purpose of the present invention is mainly achieved through the following technical solutions.

[0008] The present invention provides a method for separating rhenium and molybdenum by using a quaternary phosphine salt modified material, comprising the following steps:

[0009] 1) adding a quaternary phosphonium salt modified material to a solution containing rhenium and molybdenum, or injecting the solution into the quaternary phosphonium salt modified material, and adjusting the pH value of the solution so that the quaternary phosphonium salt modified material selectively adsorbs rhenium;

[0010] 2) After adsorption, the rhenium loaded on the material is eluted with an eluent, and the rhenium is recovered by concentration and separation, and the material is regenerated at the same time.

[0011] Preferably, the pH value in step 1) is less than 2.

[0012] Preferably, rhenium is present in the solution as ReO4 - Exists in anionic form.

[0013] For example, the quaternary phosphonium salt modified material is obtained by: firstly grafting an unsaturated monomer containing an epoxy group, a halogen, and a benzyl group onto the surface of a substrate, and then further introducing a tertiary phosphonium having a general structural formula of formula (1) onto the surface of the substrate through a halogenation reaction; or directly grafting a quaternary phosphonium ionic liquid containing an unsaturated bond onto the surface of the substrate to obtain the quaternary phosphonium salt modified material;

[0014]

[0015] Wherein, R1, R2, and R3 are alkyl, benzene ring or benzyl.

[0016] As an example, the tertiary phosphonium is selected from the following: trimethylphosphonium bromide, triethylphosphine, tri(2,4,6-trimethylphenyl)phosphine, tetraphenylphosphonium chloride, tetramethylphosphonium iodide, triphenylmethylphosphonium bromide, triphenylmethylphosphonium chloride, triphenylethylphosphonium iodide, triphenyl(2-hydroxyethyl)phosphonium chloride, triphenylethylphosphonium bromide, tri(isopropyl)phosphonium, tri(p-tolyl)phosphonium sulfate, tri(n-butyl)phosphonium sulfonate, tetra-n-butylphosphonium bromide, tetraethylphosphonium chloride, tetraethylphosphonium bromide, tetrabenzylphosphonium chloride, tetrabenzylphosphonium bromide, tetrapropylphosphonium bromide, tetrapropylphosphonium chloride. As an example, the grafting is ionizing radiation grafting or chemical grafting.

[0017] As an example, the substrate is selected from: cellulose, chitosan, lignin, chitosan and other natural polymers and their derivatives, polyethylene, polypropylene, polystyrene, polystyrene-divinylbenzene copolymer, ethylene-vinyl alcohol copolymer, polyamide and other synthetic polymers; or (nano) silica, titanium dioxide, Mxene, graphene and other inorganic materials.

[0018] By way of example, the unsaturated monomers containing epoxy groups, halogens, and benzyl groups for modifying the substrate include, but are not limited to, glycidyl acrylate (GA), glycidyl methacrylate (GMA), epichlorohydrin, allyl alcohol glycidyl ether, vinyl chloride, tetrafluoroethylene, 4-vinyl-benzyl chloride, 4-vinyl-benzyl bromide, 4-vinyl-benzyl iodide, 4-propenyl-benzyl chloride, 4-butenyl-benzyl chloride, 4-pentenyl-benzyl chloride, 4-propenyl-benzyl bromide, 4-butenyl-benzyl bromide, 4-pentenyl-benzyl bromide, 4-propenyl-benzyl iodide, 4-butenyl-benzyl iodide, and one or more of 4-pentenyl-benzyl iodide; preferably, the unsaturated monomer containing benzyl groups has a structure as shown in formula (2):

[0019]

[0020] Wherein, n is an integer between 1 and 4, and X is Cl, Br or I.

[0021] The ionizing radiation grafting is preferably electron beam pre-radiation grafting, which specifically includes the following steps: using electron beam pre-radiation on the substrate surface to generate active free radicals that can be used for grafting reaction, and then adding a solution containing unsaturated monomers after deoxygenation to the activated substrate surface, and obtaining an adsorbent precursor after graft copolymerization, wherein the unsaturated monomer is the unsaturated monomer containing benzyl group having the structure of formula (2) as described above. Preferably, the unsaturated monomer is 4-vinyl-benzyl chloride (VBC), the concentration of the unsaturated monomer in the solution is 5-40wt%, the solvent in the solution is water, ethanol or methanol, and the temperature of the graft copolymerization is controlled at 40-70°C. Preferably, the total irradiation dose used in the electron beam pre-radiation is 10-200kGy.

[0022] As an example, the initiator used in the chemical grafting includes organic peroxide and azo initiator. Preferably, the organic peroxide is cyclohexanone peroxide, dibenzoyl peroxide or tert-butyl hydroperoxide. The azo initiator includes azobisisobutyronitrile or azobisisoheptanenitrile.

[0023] In some specific application scenarios, the rhenium- and molybdenum-containing solution is usually a uranium ore alkaline leaching solution or a molybdenum ore leaching solution.

[0024] As an example, the quaternary phosphonium salt modified material is in the form of microspheres and is filled in an adsorption column as a filler. A solution containing rhenium and molybdenum is injected into the adsorption column to achieve selective adsorption of rhenium.

[0025] Preferably, in step 2), 0.1-5 mol / L HNO3 or 1%-10% ammonia solution is used as eluent to elute and separate the rhenium loaded on the material to regenerate the resin. Preferably, 1.5-3.0 mol / L HNO3 or 5% ammonia solution has a better elution effect.

[0026] Compared with the prior art, the advantages of the present invention are as follows: 1) The material preparation of the present invention is simple, the raw materials are cheap and easily available, and the preparation process is environmentally friendly.

[0027] 2) By adjusting the pH value of the adsorbed solution, the quaternary phosphonium salt modified material can effectively separate rhenium and molybdenum, selectively capture rhenium, and elute the loaded rhenium with a washing solution, with high elution efficiency; after elution, the modified material can be regenerated and reused. This overcomes the technical problems of high adsorbent cost, poor reusability, complex synthesis of most nanomaterials, low adsorption capacity, and poor selectivity in the existing rhenium and molybdenum separation process.

[0028] 3) The quaternary phosphine salt modified material provided by the present invention is easy to operate for the recovery process of rhenium, can selectively capture rhenium from the leaching solution of molybdenite, and the adsorbent can be filled in the adsorption column for use, which is suitable for large-scale recovery of rhenium in industry and has wide application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Synthetic route of quaternary phosphonium salt modified cellulose adsorption resin.

[0030] Figure 2 pH adsorption experiment of binary system Mo-Re on quaternary phosphorus salt modified cellulose adsorption resin.

[0031] Figure 3 Effect of nitrate anion on the separation of molybdenum and rhenium by quaternary phosphonium salt modified cellulose adsorbent material.

[0032] Figure 4 Effect of sulfate anion on the separation of molybdenum and rhenium by quaternary phosphonium salt modified cellulose adsorbent material.

[0033] Figure 5 Effect of Phosphate Anions on the Separation of Molybdenum and Rhenium by Quaternary Phosphonium Salt Modified Cellulose Adsorbent

[0034] Figure 6 Dynamic adsorption of rhenium from molybdenite leachate by quaternary phosphite-modified cellulose adsorption resin.

[0035] Figure 7 Dynamic desorption of rhenium from molybdenite leachate by quaternary phosphonium salt modified cellulose adsorption resin.

[0036] Figure 8 pH adsorption experiment of binary system Mo-Re on triphenylphosphine modified silica adsorbent material. DETAILED DESCRIPTION

[0037] In order to highlight the purpose, technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, after reading the content of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of the present application.

[0038] Based on the method of the present invention, taking uranium ore and molybdenite leachate as an example, the specific operation can be divided into an adsorption process and an elution process. Specifically, a quaternary phosphonium salt modified material is added to the leachate to adsorb rhenium (or the rhenium-containing solution is flowed into an adsorption column filled with a quaternary phosphonium salt modified material through a peristaltic pump); after the adsorption is completed, the corresponding eluent is used to elute and separate the rhenium loaded on the material.

[0039] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0040] Example 1 Synthesis of quaternary phosphonium salt modified cellulose adsorption resin I

[0041] The synthetic route of quaternary phosphonium salt modified cellulose adsorption resin is as follows Figure 1 shown.

[0042] First, 10.00 g of cellulose microsphere substrate was vacuum sealed and 60 Co source-γ ray irradiation (dose rate 440Gy / min, total dose 40kGy) to produce active free radicals that can be used for grafting reaction. Then, a 10wt% methanol solution of 4-vinyl-benzyl chloride after deoxygenation is added to the activated cellulose microspheres, and graft copolymerization is carried out in a vibrator at 40°C. The reaction time is 5h, and an adsorbent precursor is obtained (the grafting rate of 4-vinyl-benzyl chloride is 77%). Then, 10.00g of the adsorbent precursor is added to a 150mL polytetrafluoroethylene reactor containing 20.0g triphenylphosphine and 50mL acetone, sealed and heated to 60°C, reacted for 2 days, and a solvent thermal reaction is carried out. Finally, the cellulose resin obtained above is mixed with NaHCO3 and shaken at 40°C for 2 days to hydrolyze the residual chloromethyl groups. The microspheres are soaked in 1.5M HNO3 for 3 days to complete ion exchange and obtain a quaternary phosphonium salt modified cellulose adsorption resin. Finally, the molar content of quaternary phosphonium functional groups was 1.2 mmol / g.

[0043] Example 2 Synthesis of quaternary phosphorus salt modified cellulose adsorption resin II

[0044] The method was consistent with the synthesis method of Example 1, except that the grafting time of 4-ethylene-benzyl chloride was changed from 5 h to 24 h. The grafting rate of 4-ethylene-benzyl chloride was 132%, and the molar content of the quaternary phosphonium functional group was 1.4 mmol / g.

[0045] Example 3 Adsorption of Mo-Re Binary System by Quaternary Phosphonium Salt Modified Cellulose Adsorption Resin at Different pH

[0046] Ammonium molybdate tetrahydrate and potassium perrhenate were used to prepare a Mo-Re mixed solution, so that the concentrations of Mo and Re in the mixed solution were both 20 mg / L. Weigh 0.01 g of the adsorption resin prepared in Example 1 and put it into 10 mL of the above Mo-Re mixed solution at 30°C for a static Batch adsorption experiment. Use 0.1 mol / L HCl and NaOH to adjust the pH of the solution to 1-12, respectively, or use concentrated hydrochloric acid to prepare a mixed solution with a hydrochloric acid concentration of 1M or 3M, and conduct an adsorption experiment. After adsorption for a period of time, filter out the supernatant with a filter head, detect the concentration of metal ions with ICP-OES, and calculate its adsorption efficiency.

[0047] The pH adsorption experiment of quaternary phosphorus salt modified cellulose adsorption resin on binary system Mo-Re is as follows Figure 2 As shown in the figure, it can be concluded that under high acid conditions and when pH < 2, quaternary phosphonium salt-modified cellulose adsorption resin can selectively adsorb rhenium.

[0048] Example 4 Adsorption of Mo-Re Binary System by Quaternary Phosphonium Salt Modified Cellulose Adsorption Resin at Different Nitrate Concentrations

[0049] Weigh 0.01 g of the adsorption resin prepared in Example 1, put it into 10 mL of sodium nitrate solution containing Mo-Re at 30°C, and conduct static Batch adsorption experiments with the molar concentration ratio of Mo-Re to nitrate (the concentrations of Mo and Re remain unchanged, and the concentration of nitrate is changed) of 1.1, 1:10, 1:100, and 1:1000. Use 0.1 mol / L HCl and NaOH to adjust the pH of the solution to 1, and conduct adsorption experiments. Use a sodium nitrate solution of the same concentration without adding Mo-Re as a blank comparison. After adsorption for a period of time, filter out the supernatant with a filter head, detect the concentration of metal ions with ICP-OES, and calculate its adsorption efficiency.

[0050] The pH adsorption experiment of the binary system Mo-Re by the quaternary phosphonium salt modified cellulose adsorption resin is shown in Figure 3. It can be concluded from the figure that with the increase of nitrate concentration, the quaternary phosphonium salt modified cellulose adsorption resin can still selectively adsorb rhenium.

[0051] Example 5 Adsorption of Mo-Re Binary System by Quaternary Phosphonium Salt Modified Cellulose Adsorption Resin at Different Sulfate Concentrations

[0052] Adopting the adsorption steps similar to those in Example 4, the adsorption resin prepared in Example 1 was also used for the experiment, and the molar concentration ratio of Mo-Re to sulfate (the concentrations of Mo and Re remained unchanged, and the sulfate concentration was changed) was kept at 1:1, 1:10, 1:100, and 1:1000, and a static Batch adsorption experiment was performed. The pH of the solution was adjusted to 1 using 0.1 mol / L HCl and NaOH, and the adsorption experiment was performed. A sulfate solution of the same concentration without adding Mo-Re was used as a blank comparison. After a period of adsorption, the supernatant was filtered out with a filter head, the concentration of metal ions was detected by ICP-OES, and its adsorption efficiency was calculated.

[0053] The pH adsorption experiment of the quaternary phosphine salt modified cellulose adsorption resin on the binary system Mo-Re is shown in Figure 4. It can be concluded from the figure that the quaternary phosphine salt modified cellulose adsorption resin can selectively adsorb rhenium; even if the sulfate concentration reaches 1000 times that of Mo-Re, its adsorption efficiency for rhenium remains above 80%.

[0054] Example 6 Adsorption of Mo-Re Binary System by Quaternary Phosphonium Salt Modified Cellulose Adsorption Resin at Different Phosphate Concentrations

[0055] Adopting the adsorption steps similar to those in Example 4, the adsorption resin prepared in Example 1 was also used for the experiment, and the molar concentration ratio of Mo-Re to phosphate (the concentrations of Mo and Re remained unchanged, and the phosphate concentration was changed) was kept at 1:1, 1:10, 1:100, and 1:1000, and a static Batch adsorption experiment was performed. The pH of the solution was adjusted to 1 using 0.1 mol / L HCl and NaOH, and the adsorption experiment was performed. A phosphate solution of the same concentration without adding Mo-Re was used as a blank comparison. After a period of adsorption, the supernatant was filtered out with a filter head, the concentration of metal ions was detected by ICP-OES, and its adsorption efficiency was calculated.

[0056] The pH adsorption experiment of the binary system Mo-Re by the quaternary phosphonium salt modified cellulose adsorption resin is shown in Figure 5. It can be concluded from the figure that even if the phosphate concentration reaches 1000 times that of Mo-Re, the quaternary phosphonium salt modified cellulose adsorption resin can still selectively adsorb rhenium.

[0057] Example 7 Dynamic adsorption experiment of rhenium from molybdenite leaching solution using quaternary phosphonium salt modified cellulose adsorption resin

[0058] The quaternary phosphonium salt modified cellulose adsorption resin prepared in Example 1 was filled into the adsorption column in a wet state, and the molybdenum ore leachate was pumped into the adsorption column. Dynamic adsorption evaluation conditions: the adsorption column volume was 1 mL, and 0.45 g of quaternary phosphonium salt modified cellulose adsorption resin was filled. The molybdenum ore leachate containing Re was simulated, and the Re concentration was 0.1 mmol / L, the Mo concentration was 0.1 mmol / L, the acidity was 1M HCl, the flow rate was 0.499 mL / min, and the ratio of the volume of the solution flowing through the adsorption column to the volume of the adsorption column per unit time was SV = 20h -1 .

[0059] According to the above conditions, a dynamic adsorption evaluation experiment was carried out to obtain the adsorption behavior curve of the above adsorption material, such as Figure 6 The results show that the quaternary phosphonium salt modified cellulose adsorption resin basically does not adsorb coexisting ions in the dynamic experiment, but can selectively adsorb Re in the leachate.

[0060] Example 8 Dynamic Elution Experiment of Rhenium Recovered from Molybdenite Leachate Supported on Quaternary Phosphonium Salt Modified Cellulose Adsorption Resin

[0061] 3 mol / L HNO3 was used as the eluent to elute the rhenium-loaded quaternary phosphonium salt-modified cellulose adsorption resin in Example 7. Figure 7 It can be seen from the desorption experimental results that only 50 mL of eluent is needed to achieve an elution rate of more than 99%.

[0062] Example 9 Adsorption of Mo-Re Binary System by Triphenylphosphine-Modified Silica Adsorbent Material at Different pH

[0063] 5g SiO2, 5mL 3-(isobutylene acyloxy)propyltrimethoxysilane, and 45mL toluene were mixed and poured into a stainless steel reactor equipped with a polytetrafluoroethylene liner, and reacted in an oven at 120°C for 24h to obtain alkylated silica. Then, 1g of alkylated silica was placed in a polyethylene bag and vacuum-sealed, irradiated with 160kGy, and the deoxygenated VBC solution was injected into the polyethylene bag and sealed to prepare a VBC intermediate. Finally, 1g of VBC intermediate, 2g of triphenylphosphine and 5mL of acetone were mixed and added to a stainless steel reactor lined with polytetrafluoroethylene, heated to 60°C for 48h, and the resulting product was washed with acetone and deionized water and dried to obtain a triphenylphosphine-modified silica adsorbent material.

[0064] Weigh 0.01g of triphenylphosphine-modified silica adsorbent material and put it into 10mL of Mo-Re mixed solution (100ppm Mo, 1ppm Re) at 30℃ for static adsorption experiment. Use 0.1mol / L HCl and NaOH to adjust the pH of the solution to 1-12, or use concentrated hydrochloric acid to prepare a mixed solution with a hydrochloric acid concentration of 1M or 3M for adsorption experiment. After adsorption for a period of time, filter out the supernatant with a filter head, detect the concentration of molybdenum and rhenium with ICP-OES, and calculate its adsorption efficiency.

[0065] pH adsorption experiment of triphenylphosphine modified silica adsorbent on binary system Mo-Re Figure 8 As shown in the figure, it can be concluded that when pH < 1, even if the concentration of molybdenum is 100 times that of rhenium, the triphenylphosphine-modified silica adsorbent material basically does not adsorb molybdenum, but can selectively adsorb low-concentration rhenium.

[0066] Although the preferred embodiments of the present invention have been listed above, they are not intended to limit the contents of the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the main spirit and content of the present invention. Therefore, the scope of protection of the invention should be based on the actual scope of the claims of the patent application.

Claims

1. A method for separating rhenium and molybdenum using a quaternary phosphonium salt modified material, characterized in that: The following steps are involved: 1) adding a quaternary phosphonium salt modified material to a solution containing rhenium and molybdenum, or injecting the solution into the quaternary phosphonium salt modified material, and adjusting the pH value of the solution so that the quaternary phosphonium salt modified material selectively adsorbs rhenium; 2) After adsorption, the rhenium loaded on the material is eluted with an eluent, and the rhenium is recovered by concentration and separation, and the material is regenerated at the same time.

2. The method according to claim 1, characterized in that The quaternary phosphonium salt modified material is obtained by: firstly grafting an unsaturated monomer containing an epoxy group, a halogen, and a benzyl group onto the surface of a substrate, and then further introducing a tertiary phosphonium having a general structural formula (1) onto the surface of the substrate through a halogenation reaction; or directly grafting a quaternary phosphonium ionic liquid containing an unsaturated bond onto the surface of the substrate to obtain the quaternary phosphonium salt modified material; Wherein, R1, R2, and R3 are alkyl, benzene ring or benzyl.

3. The method according to claim 1, characterized in that The tertiary phosphonium is selected from the following: trimethylphosphonium bromide, triethylphosphine, tri(2,4,6-trimethylphenyl)phosphine, tetraphenylphosphonium chloride, tetramethylphosphonium iodide, triphenylmethylphosphonium bromide, triphenylmethylphosphonium chloride, triphenylethylphosphonium iodide, triphenyl(2-hydroxyethyl)phosphonium chloride, triphenylethylphosphonium bromide, tri(isopropyl)phosphonium, tri(p-tolyl)phosphonium sulfate, tri(n-butyl)phosphonium sulfonate, tetra-n-butylphosphonium bromide, tetraethylphosphonium chloride, tetraethylphosphonium bromide, tetrabenzylphosphonium chloride, tetrabenzylphosphonium bromide, tetrapropylphosphonium bromide, tetrapropylphosphonium chloride; The substrate is selected from: cellulose, chitosan and its derivatives, lignin and its derivatives, chitin and its derivatives, polyethylene, polypropylene, polystyrene, polystyrene-divinylbenzene copolymer, ethylene-vinyl alcohol copolymer, polyamide; or silicon dioxide, titanium dioxide, Mxene, graphene; Unsaturated monomers containing epoxy groups, halogens, and benzyl groups for modifying the substrate include, but are not limited to, one or more of glycidyl acrylate (GA), glycidyl methacrylate (GMA), epichlorohydrin, allyl alcohol glycidyl ether, vinyl chloride, tetrafluoroethylene, 4-vinyl-benzyl chloride, 4-vinyl-benzyl bromide, 4-vinyl-benzyl iodide, 4-propenyl-benzyl chloride, 4-butenyl-benzyl chloride, 4-pentenyl-benzyl chloride, 4-propenyl-benzyl bromide, 4-butenyl-benzyl bromide, 4-pentenyl-benzyl bromide, 4-propenyl-benzyl iodide, 4-butenyl-benzyl iodide, and 4-pentenyl-benzyl iodide.

4. The method according to claim 1 or 2, characterized in that: The grafting is ionizing radiation grafting or chemical grafting.

5. The method according to claim 4, characterized in that The ionizing radiation grafting is electron beam pre-radiation grafting, which specifically comprises the following steps: pre-radiating the substrate surface with an electron beam to generate active free radicals that can be used for grafting reaction, adding a deoxygenated solution containing unsaturated monomers to the activated substrate surface, and obtaining an adsorbent precursor after graft copolymerization, wherein the unsaturated monomer is an unsaturated monomer containing benzyl having a structure of formula (2): Wherein, n is an integer between 1 and 4, and X is Cl, Br or I.

6. The method according to claim 5, characterized in that The unsaturated monomer is 4-vinyl-benzyl chloride, the concentration of the unsaturated monomer in the solution is 5-40wt%, the solvent in the solution is water, ethanol or methanol, the temperature of the graft copolymerization is controlled at 40-70°C, and the total irradiation dose used in the electron beam pre-irradiation is 10-200kGy.

7. The method according to claim 4, characterized in that The initiators used in the chemical grafting include organic peroxides and azo initiators.

8. The method according to claim 7, characterized in that The organic peroxide is cyclohexanone peroxide, dibenzoyl peroxide or tert-butyl hydroperoxide. The azo initiator includes azobisisobutyronitrile or azobisisoheptanenitrile.

9. The method according to claim 1 or 2, characterized in that: In step 2), 0.1-5 mol / L HNO3 or 1%-10% ammonia solution is used as eluent to elute and separate the rhenium loaded on the material to regenerate the resin.

10. The method according to claim 1 or 2, characterized in that: Rhenium is present in the solution as ReO4 - Exists in anionic form.

Citation Information

Patent Citations

  • Quaternary phosphonium carbon nanotube material for adsorbing and separating nuclide Re / Tc as well as preparation method and application of quaternary phosphonium carbon nanotube material

    CN117797761A