Lightweight 6-series aluminum alloy and preparation method thereof

By optimizing the composition and process of 6-series aluminum alloys, a more stable aluminum alloy structure is formed, which solves the problem that 6-series aluminum alloys in the prior art is difficult to take into account both strength and lightweight, and achieves a balance between strength and lightweight, and improves the material performance of use.

CN118932223AInactive Publication Date: 2024-11-12GUANGYA ALUMINUM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997156.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure BDA0004960554900000101
    Figure BDA0004960554900000101
  • Figure BDA0004960554900000111
    Figure BDA0004960554900000111
Patent Text Reader

Abstract

The invention discloses a lightweight 6-series aluminum alloy and a preparation method thereof, and belongs to the field of aluminum alloy preparation. The light-weight 6-series aluminum alloy is prepared from the following components in percentage by mass: 0.5 percent to 0.55 percent of Si, 0.01 percent to 0.07 percent of Fe, 0.03 percent to 0.07 percent of Cu, 0.05 percent to 0.09 percent of Mn, 0.55 percent to 0.65 percent of Mg, 0.1 percent to 0.12 percent of Zn, 0.02 percent to 0.09 percent of Ti, 0.15 percent to 0.21 percent of Cr and 0.1 percent to 0.9 percent of rare earth elements. By optimizing the components and the process of the 6-series aluminum alloy, the problem that the aluminum alloy structure components are not uniform can be effectively solved, the atomic diffusivity is improved, a more stable state is presented, the components are uniformly dissolved in an aluminum matrix, the internal defects of the aluminum alloy can be reduced, the strength of the aluminum alloy material can be improved, and in aluminum profiles of the same type, the strength of the aluminum alloy material can be improved. The aluminum alloy can be lighter while the using performance is guaranteed, and the using requirement is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation of aluminum alloys, and in particular to a lightweight 6-series aluminum alloy and a preparation method thereof. Background Art

[0002] Aluminum alloy is the most widely used type of non-ferrous metal structural material in industry, and is highly favored in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. In the automobile manufacturing industry, important automobile parts are required to meet the requirements of lightweight as much as possible while meeting the mechanical properties. For automobile parts, the method of achieving lightweight in the prior art is to optimize the structure of automobile parts on the one hand, but automobiles also have certain requirements for styling, and structural optimization is relatively limited by actual production; on the other hand, the material is optimized to improve the density of the internal structure of the aluminum alloy. For example, the Chinese patent No. 201410213392.X discloses an Al-Zn-Mg-Cu aluminum alloy for automobile anti-collision beams and a method for manufacturing the product, providing a new alloy formula to improve the strength and toughness of aluminum alloy extrusions. For example, the Chinese patent No. 201710682641.3 discloses a high-performance and low-cost aluminum alloy for automobile anti-collision beams and its preparation process, wherein the aluminum alloy is subjected to a hot extrusion treatment at 440-480°C, and then a local line water mist treatment is performed at the outlet to shape the extruded material for the anti-collision beam. However, since automotive parts are in different environments and are easily affected by different environments, blindly pursuing lightweighting will also affect the strength of aluminum alloys. How to balance the strength and lightweight of aluminum alloys is the focus and difficulty of research. Summary of the invention

[0003] Based on this, in order to solve the problem that the 6-series aluminum alloy in the prior art cannot take into account both strength and lightness, the present invention provides a lightweight 6-series aluminum alloy and a preparation method thereof, and the specific technical scheme is as follows:

[0004] A lightweight 6 series aluminum alloy, the lightweight 6 series aluminum alloy comprising the following components in percentage by mass:

[0005] Si: 0.5%~0.55%, Fe: 0.01%~0.07%, Cu: 0.03%~0.07%, Mn: 0.05%~0.09%, Mg: 0.55%~0.65%, Zn: 0.1%~0.12%, Ti: 0.02%~0.09%, Cr: 0.15%~0.21%, rare earth elements: 0.1%~0.9%, total impurities ≤0.15%, Al: balance.

[0006] Furthermore, the rare earth element is obtained by mixing Nd, La and Pr in a mass ratio of (1-3): (1-2): (1-5).

[0007] In addition, the present application also provides a method for preparing a lightweight 6 series aluminum alloy, the preparation method comprising the following steps:

[0008] adding aluminum ingots, aluminum-iron alloys, aluminum-copper alloys, aluminum-manganese alloys, magnesium ingots, aluminum-titanium alloys, zinc, silicon and chromium into a smelting furnace for mixed smelting to obtain a molten metal A;

[0009] Adding a slag remover to the molten metal A, performing a first stirring treatment, performing a first slag removal treatment, then adding a rare earth element, performing a second stirring treatment, then adding a refining agent and introducing argon gas for refining treatment, performing a second slag removal treatment, and after standing treatment, obtaining a molten metal B;

[0010] Casting the molten metal B into an aluminum alloy ingot;

[0011] The aluminum alloy ingot is subjected to homogenization treatment at a temperature of 550° C. to 570° C. for 8 hours, and then rolled after cooling to room temperature at a rolling rate of 25% to 50%;

[0012] Extruding the aluminum alloy ingot after rolling;

[0013] The aluminum alloy after extrusion treatment is subjected to solid solution treatment, quenched with quenching liquid, and then cold treated at a temperature of -50°C to -10°C and a holding time of 2h to 5h;

[0014] The aluminum alloy after cold treatment is subjected to pre-aging treatment at a temperature of 90°C to 110°C and a holding time of 1h to 4h, and then subjected to aging treatment at a temperature of 150°C to 160°C and a holding time of 6h to 24h to obtain a lightweight 6 series aluminum alloy.

[0015] Furthermore, the smelting treatment is carried out by heating the temperature to 720°C to 750°C at a heating rate of 10°C / min to 15°C / min.

[0016] Furthermore, the first stirring treatment has a rotation speed of 500 r / min to 1000 r / min and a duration of 20 min to 35 min.

[0017] Furthermore, the rotation speed of the second stirring treatment is 500r / min to 1000r / min, intermittent ultrasonic action is applied, and the power of the ultrasonic action is 50W to 120W, the time is 45s to 55s, and the intermittent time is 20s to 30s.

[0018] Furthermore, the static treatment time is 25 minutes to 40 minutes.

[0019] Furthermore, the casting speed is 20 mm / min to 35 mm / min, the temperature is 700° C. to 720° C., and the cooling water volume is 7 m / t to 10 m / t.

[0020] Furthermore, before the extrusion process, the extrusion barrel is heated to a temperature of 420° C. to 450° C., the temperature of the aluminum alloy ingot is heated to a temperature of 500° C. to 520° C., and the extrusion speed is 7 m / min to 8 m / min.

[0021] Furthermore, the temperature of the solution treatment is 500° C. to 520° C., and the holding time is 30 min to 45 min.

[0022] The above scheme can effectively eliminate the problem of uneven composition of aluminum alloy tissue by optimizing the composition and process of 6 series aluminum alloy, improve the atomic diffusion capacity, present a more stable state, and evenly dissolve the components in the aluminum matrix, which can reduce the defects inside the aluminum alloy and help improve the strength of the aluminum alloy material. Among the same type of aluminum profiles, it can ensure the performance while making the aluminum alloy lighter to meet the use requirements. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0025] A lightweight 6-series aluminum alloy in one embodiment of the present invention includes the following components in percentage by mass:

[0026] Si: 0.5%~0.55%, Fe: 0.01%~0.07%, Cu: 0.03%~0.07%, Mn: 0.05%~0.09%, Mg: 0.55%~0.65%, Zn: 0.1%~0.12%, Ti: 0.02%~0.09%, Cr: 0.15%~0.21%, rare earth elements: 0.1%~0.9%, total impurities ≤0.15%, Al: balance.

[0027] In one embodiment, the rare earth element is obtained by mixing Nd, La and Pr in a mass ratio of (1-3): (1-2): (1-5).

[0028] In addition, the present application also provides a method for preparing a lightweight 6 series aluminum alloy, the preparation method comprising the following steps:

[0029] adding aluminum ingots, aluminum-iron alloys, aluminum-copper alloys, aluminum-manganese alloys, magnesium ingots, aluminum-titanium alloys, zinc, silicon and chromium into a smelting furnace for mixed smelting to obtain a molten metal A;

[0030] Adding a slag remover to the molten metal A, performing a first stirring treatment, performing a first slag removal treatment, then adding a rare earth element, performing a second stirring treatment, then adding a refining agent and introducing argon gas for refining treatment, performing a second slag removal treatment, and after standing treatment, obtaining a molten metal B;

[0031] Casting the molten metal B into an aluminum alloy ingot;

[0032] The aluminum alloy ingot is subjected to homogenization treatment at a temperature of 550° C. to 570° C. for 8 hours, and then rolled after cooling to room temperature at a rolling rate of 25% to 50%;

[0033] Extruding the aluminum alloy ingot after rolling;

[0034] The aluminum alloy after extrusion treatment is subjected to solid solution treatment, quenched with quenching liquid, and then cold treated at a temperature of -50°C to -10°C and a holding time of 2h to 5h;

[0035] The aluminum alloy after cold treatment is subjected to pre-aging treatment at a temperature of 90°C to 110°C and a holding time of 1h to 4h, and then subjected to aging treatment at a temperature of 150°C to 160°C and a holding time of 6h to 24h to obtain a lightweight 6 series aluminum alloy.

[0036] In one embodiment, the smelting process is heated to 720°C to 750°C at a heating rate of 10°C / min to 15°C / min.

[0037] In one of the embodiments, the amount of the slag remover added is (0.1-0.3) kg / t aluminum.

[0038] In one embodiment, the first stirring treatment is performed at a rotation speed of 500 r / min to 1000 r / min and for a time of 20 min to 35 min.

[0039] In one of the embodiments, the amount of the refining agent added is (0.5-0.9) kg / t aluminum.

[0040] In one embodiment, the rotation speed of the second stirring treatment is 500r / min~1000r / min, intermittent ultrasonic treatment is applied, and the power of the ultrasonic treatment is 50W~120W, the time is 45s~55s, and the intermittent time is 20s~30s.

[0041] In one embodiment, the refining treatment time is 20 minutes to 40 minutes.

[0042] In one embodiment, the static treatment time is 25 minutes to 40 minutes.

[0043] In one of the embodiments, the casting speed is 20 mm / min to 35 mm / min, the temperature is 700° C. to 720° C., and the cooling water volume is 7 m / t to 10 m / t.

[0044] In one of the embodiments, the extrusion barrel is heated to 420°C to 450°C before the extrusion process, the temperature of the aluminum alloy ingot is heated to 500°C to 520°C, and the extrusion speed is 7m / min to 8m / min.

[0045] In one embodiment, the temperature of the solution treatment is 500°C to 520°C, and the holding time is 30min to 45min.

[0046] The above scheme can effectively eliminate the problem of uneven composition of aluminum alloy tissue by optimizing the composition and process of 6 series aluminum alloy, improve the atomic diffusion capacity, present a more stable state, and evenly dissolve the components in the aluminum matrix, which can reduce the defects inside the aluminum alloy and help improve the corrosion resistance and strength of the aluminum alloy material. Among the same type of aluminum profiles, it can ensure the performance while making the aluminum alloy lighter to meet the use requirements.

[0047] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0048] Embodiment 1:

[0049] A lightweight 6 series aluminum alloy includes the following components in percentage by mass:

[0050] Si: 0.55%, Fe: 0.05%, Cu: 0.07%, Mn: 0.06%, Mg: 0.55%, Zn: 0.1%, Ti: 0.05%, Cr: 0.17%, rare earth elements: 0.9%, total impurity amount ≤ 0.15%, Al: balance; wherein the rare earth elements are obtained by mixing Nd, La and Pr in a mass ratio of 3:1:5;

[0051] A method for preparing a lightweight 6 series aluminum alloy comprises the following steps:

[0052] Aluminum ingots, aluminum-iron alloys, aluminum-copper alloys, aluminum-manganese alloys, magnesium ingots, aluminum-titanium alloys, zinc, silicon and chromium are added into a smelting furnace and heated to 750° C. at a heating rate of 10° C. / min for mixed smelting to obtain molten metal A;

[0053] According to the addition amount of 0.3kg of slag remover / ton of aluminum, a slag remover is added to the molten metal A, and the first stirring treatment is carried out at a speed of 1000r / min for 20min, the first slag removal treatment is carried out, and then rare earth elements are added, and the second stirring treatment is carried out, and the speed of the second stirring treatment is 800r / min, and intermittent ultrasonic action is applied, and the power of the ultrasonic action is 60W, the time is 45s, and the intermittent time is 20s, and then a refining agent is added in an amount of 0.6kg of refining agent / ton of aluminum, and argon gas is introduced for refining treatment for 30min, the second slag removal treatment is carried out, and after standing treatment for 30min, a molten metal B is obtained;

[0054] Casting the molten metal B into an aluminum alloy ingot at a casting speed of 20 mm / min, a temperature of 720° C., and a cooling water volume of 7 m / t;

[0055] The aluminum alloy ingot is homogenized at a temperature of 550° C. for 8 hours, and then rolled at a rolling rate of 25% after cooling to room temperature.

[0056] The aluminum alloy ingot after the rolling process is subjected to an extrusion process, and before the extrusion process, the extrusion barrel is heated to 450° C., the temperature of the aluminum alloy ingot is heated to 520° C., and the extrusion speed is 7 m / min;

[0057] The extruded aluminum alloy was solution treated at 520°C for 30 minutes, quenched with quenching liquid, and then cold treated at -50°C for 3 hours.

[0058] The aluminum alloy after cold treatment is subjected to pre-aging treatment at a temperature of 90°C and a holding time of 3 hours, and then subjected to aging treatment at a temperature of 150°C and a holding time of 10 hours to obtain a lightweight 6 series aluminum alloy.

[0059] Embodiment 2:

[0060] A lightweight 6 series aluminum alloy includes the following components in percentage by mass:

[0061] Si: 0.5%, Fe: 0.07%, Cu: 0.07%, Mn: 0.08%, Mg: 0.60%, Zn: 0.11%, Ti: 0.05%, Cr: 0.19%, rare earth elements: 0.9%, total impurity amount ≤ 0.15%, Al: balance; wherein the rare earth elements are obtained by mixing Nd, La and Pr in a mass ratio of 2:2:5;

[0062] A method for preparing a lightweight 6 series aluminum alloy comprises the following steps:

[0063] Aluminum ingots, aluminum-iron alloys, aluminum-copper alloys, aluminum-manganese alloys, magnesium ingots, aluminum-titanium alloys, zinc, silicon and chromium are added into a smelting furnace and heated to 730° C. at a heating rate of 12° C. / min for mixed smelting to obtain molten metal A;

[0064] According to the addition amount of 0.3kg of slag remover / ton of aluminum, a slag remover is added to the molten metal A, and the first stirring treatment is carried out at a speed of 1000r / min for 30min, the first slag removal treatment is carried out, and then rare earth elements are added, and the second stirring treatment is carried out, and the speed of the second stirring treatment is 1000r / min, and intermittent ultrasonic action is applied, and the power of the ultrasonic action is 50W, the time is 45s, and the intermittent time is 30s, and then a refining agent is added in an amount of 0.6kg of refining agent / ton of aluminum, and argon gas is introduced for refining treatment for 30min, the second slag removal treatment is carried out, and after standing treatment for 35min, a molten metal B is obtained;

[0065] Casting the molten metal B into an aluminum alloy ingot at a casting speed of 22 mm / min, a temperature of 720° C., and a cooling water volume of 8 m / t;

[0066] The aluminum alloy ingot is subjected to homogenization treatment at a temperature of 560° C. for 8 hours, and then rolled after cooling to room temperature at a reduction rate of 25%.

[0067] The aluminum alloy ingot after the rolling process is subjected to an extrusion process, and before the extrusion process, the extrusion barrel is heated to 430° C., the temperature of the aluminum alloy ingot is heated to 510° C., and the extrusion speed is 7 m / min;

[0068] The aluminum alloy after extrusion treatment was solution treated at a temperature of 510°C for 30 minutes, quenched with a quenching liquid, and then cold treated at a temperature of -50°C and a holding time of 3 hours;

[0069] The aluminum alloy after cold treatment is subjected to pre-aging treatment at a temperature of 100°C and a holding time of 2 hours, and then subjected to aging treatment at a temperature of 160°C and a holding time of 8 hours to obtain a lightweight 6 series aluminum alloy.

[0070] Embodiment 3:

[0071] A lightweight 6 series aluminum alloy includes the following components in percentage by mass:

[0072] Si: 0.52%, Fe: 0.06%, Cu: 0.07%, Mn: 0.08%, Mg: 0.60%, Zn: 0.11%, Ti: 0.07%, Cr: 0.18%, rare earth elements: 0.9%, total impurity amount ≤ 0.15%, Al: balance; wherein the rare earth elements are obtained by mixing Nd, La and Pr in a mass ratio of 3:2:4;

[0073] A method for preparing a lightweight 6 series aluminum alloy comprises the following steps:

[0074] Aluminum ingots, aluminum-iron alloys, aluminum-copper alloys, aluminum-manganese alloys, magnesium ingots, aluminum-titanium alloys, zinc, silicon and chromium are added into a smelting furnace and heated to 750° C. at a heating rate of 15° C. / min for mixed smelting to obtain molten metal A;

[0075] According to the addition amount of 0.3kg of slag remover / ton of aluminum, a slag remover is added to the molten metal A, and the first stirring treatment is carried out at a speed of 900r / min for 30min, the first slag removal treatment is carried out, and then rare earth elements are added, and the second stirring treatment is carried out, and the speed of the second stirring treatment is 1000r / min, and intermittent ultrasonic action is applied, and the power of the ultrasonic action is 50W, the time is 45s, and the intermittent time is 20s, and then a refining agent is added in an amount of 0.6kg of refining agent / ton of aluminum, and argon gas is introduced for refining treatment for 30min, the second slag removal treatment is carried out, and after standing treatment for 30min, a molten metal B is obtained;

[0076] Casting the molten metal B into an aluminum alloy ingot at a casting speed of 25 mm / min, a temperature of 720° C., and a cooling water volume of 7 m / t;

[0077] The aluminum alloy ingot is subjected to homogenization treatment at a temperature of 560° C. for 8 hours, and then rolled after cooling to room temperature at a reduction rate of 25%.

[0078] The aluminum alloy ingot after the rolling process is subjected to an extrusion process, and before the extrusion process, the extrusion barrel is heated to 430° C., the temperature of the aluminum alloy ingot is heated to 500° C., and the extrusion speed is 7 m / min;

[0079] The extruded aluminum alloy was solution treated at 500°C for 35 minutes, quenched with quenching liquid, and then cold treated at -50°C for 3 hours.

[0080] The aluminum alloy after cold treatment is subjected to pre-aging treatment at a temperature of 110°C and a holding time of 2 hours, and then subjected to aging treatment at a temperature of 150°C and a holding time of 6 hours to obtain a lightweight 6 series aluminum alloy.

[0081] Comparative Example 1:

[0082] The difference between Comparative Example 1 and Example 3 is that the mass percentage of the 6-series aluminum alloy in Comparative Example 1 is as follows, and the others are the same as Example 3:

[0083] Si: 0.52%, Fe: 0.06%, Cu: 0.07%, Mn: 0.08%, Mg: 0.60%, Zn: 0.11%, Ti: 0.07%, Cr: 0.18%, total impurities ≤ 0.15%, Al: balance.

[0084] Comparative Example 2:

[0085] The difference between Comparative Example 2 and Example 3 is that the mass percentage of the 6-series aluminum alloy in Comparative Example 2 is as follows, and the rest is the same as Example 3:

[0086] Si: 0.12%, Fe: 0.15%, Cu: 0.1%, Mn: 0.08%, Mg: 0.75%, Zn: 0.23%, Ti: 0.27%, Cr: 0.01%, rare earth elements: 0.3%, total impurity amount ≤0.15%, Al: balance; wherein the rare earth elements are obtained by mixing Nd, La and Pr in a mass ratio of 1:1:1.

[0087] Comparative Example 3:

[0088] The difference between Comparative Example 3 and Example 3 is that the mass percentage of the 6-series aluminum alloy in Comparative Example 3 is as follows, and the rest is the same as Example 3:

[0089] Si: 0.58%, Fe: 0.12%, Cu: 0.17%, Mn: 0.08%, Mg: 0.62%, Zn: 0.15%, Ti: 0.07%, Cr: 0.18%, La: 0.2%, total impurities ≤ 0.15%, Al: balance.

[0090] Comparative Example 4:

[0091] The difference between Comparative Example 4 and Example 3 is that no ultrasonic effect is added in Comparative Example 4, and the rest is the same as Example 3.

[0092] Comparative Example 5:

[0093] The difference between Comparative Example 5 and Example 3 is that Comparative Example 5 is not subjected to rolling treatment, and the rest is the same as Example 3.

[0094] Comparative Example 6:

[0095] The difference between Comparative Example 6 and Example 3 is that Comparative Example 6 is not subjected to cold treatment, and the rest is the same as Example 3.

[0096] Comparative Example 7:

[0097] The difference between Comparative Example 7 and Example 3 is that Comparative Example 7 is not subjected to pre-aging treatment, and the rest is the same as Example 3.

[0098] The 6 series aluminum alloy samples prepared in Examples 1 to 3 and the 6 series aluminum alloy comparison samples prepared in Comparative Examples 1 to 7 were subjected to performance tests in accordance with the metal material tensile test standard GB / T228.1-2010 and the metal material Brinell hardness standard GB / T231.1-2009. The results are shown in Table 1 below.

[0099] Table 1: Performance results

[0100]

[0101]

[0102] From the data analysis in Table 1, it can be seen that the present application can significantly improve the strength of the 6 series aluminum alloy as a whole by optimizing the composition and component ratio of the 6 series aluminum alloy and combining the process, while ensuring the use strength of the 6 series aluminum alloy while reducing the weight to meet the use requirements.

[0103] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0104] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A lightweight 6 series aluminum alloy, characterized in that: The lightweight 6 series aluminum alloy includes the following components in mass percentage: Si: 0.5%~0.55%, Fe: 0.01%~0.07%, Cu: 0.03%~0.07%, Mn: 0.05%~0.09%, Mg: 0.55%~0.65%, Zn: 0.1%~0.12%, Ti: 0.02%~0.09%, Cr: 0.15%~0.21%, rare earth elements: 0.1%~0.9%, total impurities ≤0.15%, Al: balance.

2. The lightweight 6 series aluminum alloy according to claim 1, characterized in that: The rare earth element is obtained by mixing Nd, La and Pr in a mass ratio of (1-3): (1-2): (1-5).

3. A method for preparing a lightweight 6 series aluminum alloy, characterized in that: The preparation method is used to prepare the lightweight 6 series aluminum alloy as claimed in claim 1 or 2, and the preparation method comprises the following steps: adding aluminum ingots, aluminum-iron alloys, aluminum-copper alloys, aluminum-manganese alloys, magnesium ingots, aluminum-titanium alloys, zinc, silicon and chromium into a smelting furnace for mixed smelting to obtain a molten metal A; Adding a slag remover to the molten metal A, performing a first stirring treatment, performing a first slag removal treatment, then adding a rare earth element, performing a second stirring treatment, then adding a refining agent and introducing argon gas for refining treatment, performing a second slag removal treatment, and after standing treatment, obtaining a molten metal B; Casting the molten metal B into an aluminum alloy ingot; The aluminum alloy ingot is subjected to homogenization treatment at a temperature of 550° C. to 570° C. for 8 hours, and then rolled after cooling to room temperature at a rolling rate of 25% to 50%; Extruding the aluminum alloy ingot after rolling; The aluminum alloy after extrusion treatment is subjected to solid solution treatment, quenched with quenching liquid, and then cold treated at a temperature of -50°C to -10°C and a holding time of 2h to 5h; The aluminum alloy after cold treatment is subjected to pre-aging treatment at a temperature of 90°C to 110°C and a holding time of 1h to 4h, and then subjected to aging treatment at a temperature of 150°C to 160°C and a holding time of 6h to 24h to obtain a lightweight 6 series aluminum alloy.

4. The preparation method according to claim 3, characterized in that: The smelting process is heated to 720°C to 750°C at a heating rate of 10°C / min to 15°C / min.

5. The preparation method according to claim 3, characterized in that: The first stirring treatment has a rotation speed of 500 r / min to 1000 r / min and a time of 20 min to 35 min.

6. The preparation method according to claim 3, characterized in that: The rotation speed of the second stirring treatment is 500r / min to 1000r / min, and intermittent ultrasonic treatment is applied. The power of the ultrasonic treatment is 50W to 120W, the time is 45s to 55s, and the intermittent time is 20s to 30s.

7. The preparation method according to claim 3, characterized in that: The time of the static treatment is 25min to 40min.

8. The preparation method according to claim 3, characterized in that: The casting speed is 20 mm / min to 35 mm / min, the temperature is 700° C. to 720° C., and the cooling water volume is 7 m / t to 10 m / t.

9. The preparation method according to claim 3, characterized in that: Before the extrusion process, the extrusion barrel is heated to 420° C. to 450° C., the temperature of the aluminum alloy ingot is heated to 500° C. to 520° C., and the extrusion speed is 7 m / min to 8 m / min.

10. The preparation method according to claim 3, characterized in that: The temperature of the solution treatment is 500° C. to 520° C., and the holding time is 30 min to 45 min.