Aluminum alloy resistant to marine environment and preparation method thereof

By optimizing the composition and process parameters of aluminum alloy, the problem of poor corrosion resistance in marine environments is solved, which significantly improves corrosion resistance and mechanical properties, extends service life and reduces maintenance costs.

CN118932229AInactive Publication Date: 2024-11-12GUANGYA ALUMINUM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027302.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Aluminum alloys have poor corrosion resistance in marine environments and are prone to stress corrosion, hydrogen embrittlement, corrosion fatigue and intergranular corrosion, resulting in sudden breakage of metal structures and causing huge losses.

Method used

By optimizing the composition of aluminum alloy, adding Ce, La, Re and Zr, the amount of components is limited, the interaction between components is reduced, the grain size is reduced, and the grain growth is hindered. Through process parameters control, multi-stage Aging treatment and solid solution treatment improve the corrosion resistance of aluminum alloys.

Benefits of technology

It significantly improves the corrosion resistance and mechanical properties of aluminum alloys, extends service life, reduces maintenance costs, and makes it more suitable for marine environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968910740000071
    Figure BDA0004968910740000071
  • Figure BDA0004968910740000082
    Figure BDA0004968910740000082
  • Figure BDA0004968910740000091
    Figure BDA0004968910740000091
Patent Text Reader

Abstract

The invention discloses a marine environment resistant aluminum alloy and a preparation method thereof, and belongs to the field of aluminum alloy preparation. According to the invention, Ce, La, Re and Zr are added, and the addition amount of the components is limited, so that the components interact with one another, the crystal grains of the internal structure of the aluminum alloy are reduced, the growth of the crystal grains is effectively hindered, and the risk of intergranular corrosion is further reduced; in addition, Ce can react with hydrogen in the aluminum alloy liquid to form dispersed hydride, then the porosity in the aluminum alloy cast ingot is reduced, the structure form of the aluminum alloy is optimized, the Ce interacts with La, Re and Zr, intergranular corrosion can be effectively resisted, the mechanical performance of the aluminum alloy can be promoted, the service life of the aluminum alloy can be prolonged, and the maintenance cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aluminum alloy preparation, and in particular to an aluminum alloy resistant to marine environments and a preparation method thereof. Background Art

[0002] Aluminum alloys have excellent properties such as low density, good mechanical properties, and easy recycling. They meet the needs of modern technology for lightweight materials and are widely used in highway facilities, automobiles, rail transit, spacecraft, ships and other fields. In reports of aluminum alloy material failure in service, mold-induced corrosion failure is common, especially in the humid and hot marine environment. As an important structural material, aluminum alloys are also widely used in marine operating equipment. The marine environment is mostly rainy, with strong winds and high salt spray concentrations. Stress corrosion, hydrogen embrittlement, corrosion fatigue, intergranular corrosion, etc. caused by the corrosion of metal equipment in the ocean will lead to sudden fracture of metal structures and cause huge losses. Therefore, the corrosion resistance of aluminum alloy materials needs to be further strengthened. Summary of the invention

[0003] Based on this, in order to solve the problem of poor corrosion resistance of aluminum alloys prepared in the prior art when used in marine environments, the present invention provides an aluminum alloy resistant to marine environments and a preparation method thereof. The specific technical scheme is as follows:

[0004] A marine environment resistant aluminum alloy, comprising the following components in mass percentage: Mg: 2.1% to 3.3%, Mn: 0.2% to 0.8%, Cu: 0.03% to 0.24%, Ce: 0.05% to 0.09%, La: 0.03% to 0.12%, Re: 0.01% to 0.03%, Zr: 0.03% to 0.09%, Ti: 0.05% to 0.16%, and Zr+Ti: 0.08% to 0.25%, Si≤0.10%, single impurity≤0.05%, total impurity≤0.1%, and the balance is Al.

[0005] In addition, the present invention provides a method for preparing an aluminum alloy resistant to marine environments, the preparation method comprising the following steps:

[0006] Adding aluminum raw materials into a smelting furnace to melt and obtain aluminum liquid, then adding Cu raw materials, Ce raw materials, La raw materials, Re raw materials and Zr raw materials into the aluminum liquid, performing a first smelting process and a first slag removal process, to obtain alloy liquid A;

[0007] Mg raw material, Mn raw material, Ti raw material and Si raw material are continuously added to the alloy liquid A to perform a second smelting process and a second slag removal process to obtain alloy liquid B;

[0008] Adding a refining agent to the alloy liquid B and performing a degassing and refining treatment under an argon atmosphere, standing treatment, and then casting treatment to obtain an aluminum alloy ingot;

[0009] The aluminum alloy ingot is subjected to extrusion treatment, solution treatment and double-stage aging treatment, and then cooled by strong wind to obtain the aluminum alloy.

[0010] Furthermore, the first smelting treatment is carried out by heating the temperature to 720°C to 750°C at a heating rate of 10°C / min to 15°C / min for 30min to 50min.

[0011] Furthermore, the temperature of the first deslagging treatment is 700°C to 720°C.

[0012] Furthermore, the temperature of the second smelting treatment is 700° C. to 720° C., and the time is 20 min to 30 min.

[0013] Furthermore, the temperature of the second deslagging treatment is 710°C to 720°C.

[0014] Furthermore, the refining treatment is carried out at a temperature of 700°C to 730°C and for a time of 10 min to 20 min.

[0015] Furthermore, the casting process has a temperature of 700° C. to 720° C., a water pressure of 0.05 MPa to 0.10 MPa, and a speed of 45 mm / min to 50 mm / min.

[0016] Furthermore, the temperature of the solution treatment is 490°C to 510°C, the holding time is 50min to 60min, the quenching medium is water, and the temperature is 20°C to 25°C.

[0017] Furthermore, the two-stage aging treatment includes a primary aging treatment and a secondary aging treatment, and the primary aging treatment is heated to 150°C to 160°C at a heating rate of 1°C / min to 3°C / min and kept warm for 5h to 8h, and the secondary aging treatment is heated to 165°C to 175°C at a heating rate of 0.5°C / min to 1.5°C / min and kept warm for 4h to 5h.

[0018] In the above scheme, by optimizing the composition of aluminum alloy, adding Ce, La, Re and Zr, and limiting the addition amount of the components, the components interact with each other, the grain size of the internal structure of the aluminum alloy is reduced and the grain growth is effectively hindered, thereby reducing the risk of intergranular corrosion; Ce can also react with hydrogen in the aluminum alloy liquid to form dispersed hydrides, thereby reducing the porosity in the aluminum alloy ingot, and optimizing the organizational morphology of the aluminum alloy, interacting with La, Re and Zr, not only effectively resisting intergranular corrosion, but also promoting the mechanical properties of the aluminum alloy, helping to increase its service life and reduce maintenance costs.

[0019] In addition, the present application ensures the flow formability of the aluminum alloy and reduces the impact of corrosive media on the corrosion resistance of the aluminum alloy by controlling the process parameters in the preparation method, so that the aluminum alloy is not easily deformed and is more suitable for marine application environments. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0022] An aluminum alloy resistant to marine environments in one embodiment of the present invention comprises the following components in mass percentage: Mg: 2.1% to 3.3%, Mn: 0.2% to 0.8%, Cu: 0.03% to 0.24%, Ce: 0.05% to 0.09%, La: 0.03% to 0.12%, Re: 0.01% to 0.03%, Zr: 0.03% to 0.09%, Ti: 0.05% to 0.16%, and Zr+Ti: 0.08% to 0.25%, Si≤0.10%, single impurity≤0.05%, total impurities≤0.1%, and the balance is Al.

[0023] In addition, the present invention provides a method for preparing an aluminum alloy resistant to marine environments, the preparation method comprising the following steps:

[0024] Adding aluminum raw materials into a smelting furnace to melt and obtain aluminum liquid, then adding Cu raw materials, Ce raw materials, La raw materials, Re raw materials and Zr raw materials into the aluminum liquid, performing a first smelting process and a first slag removal process, to obtain alloy liquid A;

[0025] Mg raw material, Mn raw material, Ti raw material and Si raw material are continuously added to the alloy liquid A to perform a second smelting process and a second slag removal process to obtain alloy liquid B;

[0026] Adding a refining agent to the alloy liquid B and performing a degassing and refining treatment under an argon atmosphere, standing treatment, and then casting treatment to obtain an aluminum alloy ingot;

[0027] The aluminum alloy ingot is subjected to extrusion treatment, solution treatment and double-stage aging treatment, and then cooled by strong wind to obtain the aluminum alloy.

[0028] In one embodiment, the first smelting treatment is carried out by heating the temperature to 720°C to 750°C at a heating rate of 10°C / min to 15°C / min for 30min to 50min.

[0029] In one embodiment, the temperature of the first deslagging treatment is 700°C to 720°C.

[0030] In one embodiment, the temperature of the second smelting treatment is 700° C. to 720° C., and the time is 20 min to 30 min.

[0031] In one of the embodiments, a low-frequency electromagnetic field is further added in the second smelting process, wherein the frequency of the low-frequency electromagnetic field is 10 Hz to 20 Hz, and the magnetic field strength is 10000 A / m to 11000 A / m.

[0032] In one embodiment, the temperature of the second deslagging treatment is 710°C to 720°C.

[0033] In one embodiment, the refining treatment is carried out at a temperature of 700°C to 730°C and for a time of 10 min to 20 min.

[0034] In one embodiment, the static treatment time is 1 hour to 3 hours.

[0035] In one of the embodiments, the casting process is performed at a temperature of 700° C. to 720° C., a water pressure of 0.05 MPa to 0.10 MPa, and a speed of 45 mm / min to 50 mm / min.

[0036] In one embodiment, the extrusion process is performed at a speed of 2 m / s to 5 m / s and a pressure of 10 MPa to 20 MPa.

[0037] In one embodiment, the temperature of the solution treatment is 490°C to 510°C, the holding time is 50min to 60min, the quenching medium is water, and the temperature is 20°C to 25°C.

[0038] In one embodiment, the two-stage aging treatment includes a primary aging treatment and a secondary aging treatment, and the primary aging treatment is heated to 150°C to 160°C at a heating rate of 1°C / min to 3°C / min and kept warm for 5h to 8h, and the secondary aging treatment is heated to 165°C to 175°C at a heating rate of 0.5°C / min to 1.5°C / min and kept warm for 4h to 5h.

[0039] The aluminum alloy prepared by the above scheme has excellent corrosion resistance and can be used in marine environments.

[0040] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0041] Embodiment 1~3:

[0042] The aluminum alloys of Examples 1 to 3 have different compositions, as shown in Table 1, and the preparation processes are the same;

[0043] A method for preparing an aluminum alloy resistant to marine environments comprises the following steps:

[0044] Adding aluminum raw material into a smelting furnace to melt to obtain aluminum liquid, then adding Cu raw material, Ce raw material, La raw material, Re raw material and Zr raw material to the aluminum liquid, heating to 740° C. at a heating rate of 10° C. / min for a first smelting treatment for 45 min, and performing a first slag removal treatment at 710° C. to obtain alloy liquid A;

[0045] Mg raw material, Mn raw material, Ti raw material and Si raw material are continuously added to the alloy liquid A, and a second smelting treatment is performed for 25 minutes at 720° C., a frequency of 13 Hz and a magnetic field strength of 10000 A / m, and a second slag removal treatment is performed at 720° C. to obtain alloy liquid B;

[0046] Adding a refining agent to the alloy liquid B and performing a degassing and refining treatment at 720° C. for 15 min in an argon atmosphere, standing for 2 h, and then casting at a temperature of 720° C., a water pressure of 0.08 MPa, and a speed of 45 mm / min to obtain an aluminum alloy ingot;

[0047] The aluminum alloy ingot is subjected to extrusion treatment at a speed of 3 m / s and a pressure of 15 MPa, and then subjected to solution treatment at a temperature of 500° C. for 50 min, with the quenching medium being water and the temperature being 20° C., and then subjected to double-stage aging treatment, and the double-stage aging treatment includes primary aging treatment and secondary aging treatment, and the primary aging treatment is heated to 150° C. at a heating rate of 1° C. / min and kept warm for 6 h, and the secondary aging treatment is heated to 170° C. at a heating rate of 0.5° C. / min and kept warm for 4 h, and then the aluminum alloy is obtained after strong wind cooling.

[0048] Comparative Examples 1 to 6:

[0049] The difference between Comparative Examples 1 to 6 and Example 3 is that the components and mass percentages of the aluminum alloys are different, as shown in Table 1, and the rest are the same as Example 3.

[0050] Comparative Example 7:

[0051] The difference between Comparative Example 7 and Example 3 is that the process of Comparative Example 7 is different from that of Example 3, and the rest is the same as that of Example 3. The aluminum alloy preparation method of Comparative Example 7 includes the following steps:

[0052] A method for preparing an aluminum alloy comprises the following steps:

[0053] Adding an aluminum raw material into a smelting furnace to melt and obtain aluminum liquid, then adding a Cu raw material, a Ce raw material, a La raw material, a Re raw material, a Zr raw material, a Mg raw material, a Mn raw material, a Ti raw material and a Si raw material to the aluminum liquid, heating the temperature to 740° C. at a heating rate of 10° C. / min for smelting treatment for 1 hour, and performing a slag removal treatment at 710° C. to obtain an alloy liquid;

[0054] Adding a refining agent to the alloy liquid and performing a degassing and refining treatment at 720° C. for 15 minutes in an argon atmosphere, standing for 2 hours, and then casting at a temperature of 720° C., a water pressure of 0.08 MPa, and a speed of 45 mm / min to obtain an aluminum alloy ingot;

[0055] The aluminum alloy ingot is subjected to extrusion treatment at a speed of 3 m / s and a pressure of 15 MPa, and then subjected to solution treatment at a temperature of 500° C. for 50 min, with the quenching medium being water and the temperature being 20° C., and then subjected to double-stage aging treatment, and the double-stage aging treatment includes primary aging treatment and secondary aging treatment, and the primary aging treatment is heated to 150° C. at a heating rate of 1° C. / min and kept warm for 6 h, and the secondary aging treatment is heated to 170° C. at a heating rate of 0.5° C. / min and kept warm for 4 h, and then the aluminum alloy is obtained after strong wind cooling.

[0056] Comparative Example 8:

[0057] The difference between Comparative Example 8 and Example 3 is that the process of Comparative Example 8 is different from that of Example 3, and the other processes are the same as those of Example 3. The aluminum alloy preparation method of Comparative Example 8 includes the following steps:

[0058] A method for preparing an aluminum alloy comprises the following steps:

[0059] Adding an aluminum raw material into a smelting furnace to melt and obtain aluminum liquid, then adding a Cu raw material, a Ce raw material, a La raw material, a Re raw material, a Zr raw material, a Mg raw material, a Mn raw material, a Ti raw material and a Si raw material to the aluminum liquid, heating the temperature to 740° C. at a heating rate of 10° C. / min for smelting treatment for 1 hour, and performing a slag removal treatment at 710° C. to obtain an alloy liquid;

[0060] Adding a refining agent to the alloy liquid and performing a degassing and refining treatment at 720° C. for 15 minutes in an argon atmosphere, standing for 2 hours, and then casting at a temperature of 720° C., a water pressure of 0.08 MPa, and a speed of 45 mm / min to obtain an aluminum alloy ingot;

[0061] The aluminum alloy ingot is extruded at a speed of 3 m / s and a pressure of 15 MPa, and then solution treated at a temperature of 500°C for 50 min, with the quenching medium being water at a temperature of 20°C, and then kept at a temperature of 170°C for 6 hours, and cooled with strong wind to obtain an aluminum alloy.

[0062] Table 1: Aluminum alloy composition (%)

[0063]

[0064]

[0065] Test Example 1:

[0066] The aluminum alloy samples prepared in Examples 1 to 3 and the aluminum alloy comparison samples prepared in Comparative Examples 1 to 8 were tested for mechanical properties. The results are shown in Table 2.

[0067] Table 2: Mechanical properties

[0068]

[0069] From the data analysis of Table 2, it can be seen that the aluminum alloy prepared by the present invention has excellent mechanical properties. After the optimization of the composition, it can effectively hinder the growth of the second phase and the dissolution of other impurities, so that the grain growth trend is weakened, which is conducive to eliminating and reducing intracrystalline segregation. It has excellent organizational uniformity, is not easy to crack when bent, and has a high use value.

[0070] Test Example 2: Seawater Corrosion Resistance Simulation Test

[0071] Artificial seawater was prepared according to the standard of "ASTM D1141-98 (2013) Seawater Substitutes". The test method was carried out in accordance with "GB / T 19746-2005 Metal and Alloy Corrosion Salt Solution Cyclic Immersion Test". The test temperature was 70°C. Sampling and analysis were carried out every 5 days. The analysis method adopted spectrophotometry or other instrumental analysis methods to test the aluminum dissolution amount. The results are shown in Table 3 below.

[0072] Table 3: Aluminum dissolution (mg / L)

[0073]

[0074] From the data analysis in Table 3, it can be seen that after the composition and process of the aluminum alloy prepared in the present application are optimized, not only the mechanical properties are optimized, but also the corrosion resistance is significantly improved, making it more suitable for application in marine environments.

[0075] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An aluminum alloy resistant to marine environment, characterized in that: The aluminum alloy includes the following components in mass percentage: Mg: 2.1% to 3.3%, Mn: 0.2% to 0.8%, Cu: 0.03% to 0.24%, Ce: 0.05% to 0.09%, La: 0.03% to 0.12%, Re: 0.01% to 0.03%, Zr: 0.03% to 0.09%, Ti: 0.05% to 0.16%, and Zr+Ti: 0.08% to 0.25%, Si≤0.10%, single impurity≤0.05%, total impurities≤0.1%, and the balance is Al.

2. A method for preparing an aluminum alloy resistant to marine environments, characterized in that: The preparation method is used to prepare the aluminum alloy according to claim 1, and the preparation method comprises the following steps: Adding aluminum raw materials into a smelting furnace to melt and obtain aluminum liquid, then adding Cu raw materials, Ce raw materials, La raw materials, Re raw materials and Zr raw materials into the aluminum liquid, performing a first smelting process and a first slag removal process, to obtain alloy liquid A; Mg raw material, Mn raw material, Ti raw material and Si raw material are continuously added to the alloy liquid A to perform a second smelting process and a second slag removal process to obtain alloy liquid B; Adding a refining agent to the alloy liquid B and performing a degassing and refining treatment under an argon atmosphere, standing treatment, and then casting treatment to obtain an aluminum alloy ingot; The aluminum alloy ingot is subjected to extrusion treatment, solution treatment and double-stage aging treatment, and then cooled by strong wind to obtain the aluminum alloy.

3. The preparation method according to claim 2, characterized in that: The first smelting treatment is carried out by heating the temperature to 720°C to 750°C at a heating rate of 10°C / min to 15°C / min for 30min to 50min.

4. The preparation method according to claim 2, characterized in that: The temperature of the first deslagging treatment is 700°C to 720°C.

5. The preparation method according to claim 2, characterized in that: The temperature of the second smelting treatment is 700° C. to 720° C., and the time is 20 min to 30 min.

6. The preparation method according to claim 2, characterized in that: The temperature of the second deslagging treatment is 710°C to 720°C.

7. The preparation method according to claim 2, characterized in that: The refining treatment is carried out at a temperature of 700° C. to 730° C. and for a time of 10 min to 20 min.

8. The preparation method according to claim 2, characterized in that: The casting process is performed at a temperature of 700° C. to 720° C., a water pressure of 0.05 MPa to 0.10 MPa, and a speed of 45 mm / min to 50 mm / min.

9. The preparation method according to claim 2, characterized in that: The temperature of the solution treatment is 490°C to 510°C, the holding time is 50min to 60min, the quenching medium is water, and the temperature is 20°C to 25°C.

10. The preparation method according to claim 2, characterized in that: The two-stage aging treatment includes a primary aging treatment and a secondary aging treatment, and the primary aging treatment is heated to 150°C to 160°C at a heating rate of 1°C / min to 3°C / min and kept warm for 5h to 8h, and the secondary aging treatment is heated to 165°C to 175°C at a heating rate of 0.5°C / min to 1.5°C / min and kept warm for 4h to 5h.