High-density oxide target material and preparation method thereof

By using oxide precursor powder ratios of different particle sizes in the preparation of indium oxide targets, high-density and high-performance target preparation is achieved, the problems of low density and coarse grains are solved, and the indium oxide targets are improved conductivity and mechanical hardness.

CN118932286AActive Publication Date: 2024-11-12XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411295103.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-15
Publication Date
2024-11-12
Estimated Expiration
2044-09-15

AI Technical Summary

Technical Problem

During the sintering process, existing indium oxide targets have insufficient conductivity and mechanical hardness due to low density, coarse grains, and uneven element distribution. It is difficult to achieve high density in traditional single particle molding.

Method used

A small amount of oxide precursor powder with large particle size and large amounts of small particle size is mixed, and the particle size ratio is adjusted through molding and sintering to improve the relative density and molding effect of the target material and reduce the resistivity.

Benefits of technology

It effectively improves the relative density and molding effect of the oxide target material, reduces holes, improves the tightness and performance of the target material, and is especially suitable for high indium oxide content target materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045719600000111
    Figure BDA0005045719600000111
  • Figure BDA0005045719600000121
    Figure BDA0005045719600000121
Patent Text Reader

Abstract

The invention belongs to the technical field of new materials, and discloses a preparation method of a high-density oxide target material, which comprises the following steps: mixing first oxide precursor powder and second oxide precursor powder, carrying out compression molding, and sintering to obtain the target material, the first oxide precursor powder and the second oxide precursor powder both contain not less than 97 wt% of indium oxide; the weight of the first oxide precursor powder is equivalent to 80-90% of the total weight of the first oxide precursor powder and the second oxide precursor powder; the particle size of the first oxide precursor powder is 20-30 [mu] m; and the particle size of the second oxide precursor powder is 45-73 [mu] m. According to the method, a small amount of large-particle-size precursor powder and a large amount of small-particle-size precursor powder are adopted for the target material with the high indium oxide content, the relative density of the target material of the type can be effectively improved, the electrical resistivity can be effectively reduced, and the forming effect can be effectively improved. Meanwhile, the invention also provides the high-density oxide target material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials, and in particular to a high-density oxide target material and a preparation method thereof. Background Art

[0002] Indium oxide is an n-type semiconductor material with high conductivity, high transmittance (visible light band), wide bandgap, high mechanical hardness and good stability. On this basis, doping it can further improve the conductivity of the thin film material, that is, indium oxide-based TCO thin film. There are many kinds of doping elements, such as tin, tungsten, titanium, zirconium, manganese and other elements. However, the quality of indium oxide-based thin films depends to a large extent on the quality of indium oxide-based targets. At present, the sintering of targets usually requires long-term sintering at high temperatures, which can lead to problems such as coarse grains, uneven element distribution, and high energy consumption. Therefore, in order to achieve low-energy preparation of high-quality targets, it is necessary to reduce the sintering temperature by increasing the green density, thereby avoiding the occurrence of undesirable problems.

[0003] The preparation process of indium oxide-based targets is divided into three steps: powder preparation, green body forming and sintering. These three steps are key factors affecting the quality of the target. The fineness and uniformity of the powder is conducive to improving the activity of sintering, so in the process of preparing the target, powders with small particle diameters and good dispersibility are usually used. Secondly, in the powder forming process, the larger the particle diameter, the greater the friction generated, resulting in stress attenuation of the compacted target, resulting in problems such as uneven particle stacking and low density in the green body, which will ultimately affect the sintering performance of the target.

[0004] The low-density green body particles are loosely packed, and the particles are easier to rotate during sintering, so the densification rate is higher, but the density of its sintered body is still lower than that of the high-density green body; although the high green body density sample has a low densification rate, it is easier to obtain high density at a lower temperature and the grain size is small. Therefore, a high green body density is conducive to obtaining a high-density indium oxide-based target. The packing density and uniformity of the particles must be ensured during the molding process. Uneven stacking leads to shrinkage differences in the target during the sintering process, which causes holes inside the target and reduces the density of the target.

[0005] The most common forming method for green bodies is a combination of molding and cold isostatic pressing. The simplest way to increase the density of green bodies is to increase the stress of pressing the green bodies. This method will cause large internal stress in the green bodies and produce cracks during sintering. The process of green body forming is a process of particle accumulation. The size grading accumulation of powder particles is widely used in fields such as water conservancy, geology and powder metallurgy. In the preparation of ceramics, the accumulation theory is often used as the design of porous ceramics, and the theory is also used to control the grain size of ceramics. The traditional single particle method is difficult to achieve high density. The highest theoretical density of uniform spherical particles of a single size is 0.74.

[0006] In order to seek higher green compact density and subsequent sintering target density, the applicant previously filed a patent application CN116143500B for an indium oxide molybdenum praseodymium target and a preparation method thereof, which disclosed Pr6O 11 The mass ratio of powder, MoO3 powder and In2O3 powder is 10-23:5-17:60-80; the particle size of the coarse powder is 90-115μm, and the particle size of the fine powder is 10-35μm; when the particle size of the coarse powder is 90-100μm, and the particle size of the coarse powder is not 100μm, the ratio of fine powder to coarse powder is 1:6-9; when the particle size of the coarse powder is 100-105μm, and the particle size of the coarse powder is not 105μm, the ratio of fine powder to coarse powder is 1:9-12; when the particle size of the coarse powder is 105-115μm, the ratio of fine powder to coarse powder is 1:12-16. The result is: the true density is above 6.2, and the forming rate is above 80%.

[0007] Another prior application of the applicant, CN116219375B, describes an indium zinc oxide target material and a preparation method thereof: part of the indium oxide is prepared into small particles, and part of the indium oxide is prepared into large particles, the atomic ratio of large-particle indium oxide to small-particle indium oxide is 3:7-1:9; the particle size D50 of the large-particle indium oxide is 1-2μm, and D90 is 1-1.8μm, and the particle size D50 of the small-particle indium oxide is 0.1-0.3μm, and D90 is 0.1-0.2μm; then the large particles, small particles and zinc oxide are pulped and spray granulated.

[0008] The result is a relative density of more than 98% and a resistivity of less than 135;

[0009] From the above records, it can be seen that for indium oxide targets, adjusting the powder particle size or adjusting the raw material particle size can optimize density and other related properties.

[0010] We hope that the density of indium oxide targets can be further improved to reduce damage to the targets.

[0011] The technical problem solved in this case is how to further increase the relative density of indium oxide target material and improve the molding effect. Summary of the invention

[0012] The purpose of the present invention is to provide a method for preparing a high-density oxide target material. The method of the present invention is aimed at a target material with a high indium oxide content. A small amount of large-particle precursor powder and a large amount of small-particle precursor powder are used, which can effectively improve the relative density of this type of target material, reduce the resistivity, and improve the molding effect.

[0013] At the same time, the present invention also provides the high-density oxide target material.

[0014] To achieve the above objectives, this application discloses:

[0015] A method for preparing a high-density oxide target material, comprising mixing a first oxide precursor powder and a second oxide precursor powder, pressing and sintering the mixture to obtain a target material;

[0016] The first oxide precursor powder and the second oxide precursor powder both contain no less than 97 wt % of indium oxide;

[0017] The weight of the first oxide precursor powder is equivalent to 80% to 90% of the total weight of the first oxide precursor powder and the second oxide precursor powder;

[0018] The particle size of the first oxide precursor powder is 20 to 30 μm; the particle size of the second oxide precursor powder is 45 to 73 μm.

[0019] The present invention uses oxide target precursor powders of different particle sizes, adjusts the ratio of different particle sizes, and mixes small particles into large particles. As the proportion of small particles increases, the lubrication effect becomes more obvious, which can effectively solve the problems of more pores and loose particle stacking when large particle powders dominate. The preparation of high-density green billets also gradually reduces the number of target holes and the diameter of the holes is also reduced, so that the compactness of the oxide target is gradually improved.

[0020] When verifying indium oxide targets with different ratios, the present invention further found that the method is particularly effective for targets with high indium oxide content.

[0021] In the above-mentioned method for preparing a high-density oxide target, the first oxide precursor powder and the second oxide precursor powder both contain no less than 98 wt % of indium oxide.

[0022] In the above-mentioned method for preparing a high-density oxide target, the first oxide precursor powder and the second oxide precursor powder further contain one or more combinations of cerium oxide, titanium oxide, tantalum oxide, molybdenum oxide, praseodymium oxide, and zinc oxide.

[0023] In the above-mentioned method for preparing a high-density oxide target, the first oxide precursor powder and the second oxide precursor powder contain 97.5 wt % to 99.7 wt % of indium oxide.

[0024] More preferably, the first oxide precursor powder and the second oxide precursor powder both contain indium oxide powder, cerium oxide powder, titanium oxide powder and tantalum oxide powder; the weight ratio of each powder is: 97.5~99.7:0.1~1:0.1~1:0.1~0.5.

[0025] In the above-mentioned method for preparing high-density oxide target materials, the preparation methods of the first oxide precursor powder and the second oxide precursor powder are: mixing oxide, dispersant, and binder into a slurry with a solid content of 30wt% to 95wt%, and then sand grinding and spray granulation to obtain powder of corresponding particle size.

[0026] In the sand milling process of preparing the first oxide precursor powder, the grinding balls used are a mixture of three specifications of grinding balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm; the weight ratio of the grinding balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm is 4-7:1-4:1-4;

[0027] In the sand milling process of preparing the second oxide precursor powder, the grinding balls used are 0.8 mm to 1.0 mm grinding balls.

[0028] In the above-mentioned method for preparing a high-density oxide target, during the sand milling operation, the speed of the sand mill is 800 to 1600 rpm, and the grinding time is 2 to 12 hours;

[0029] During the spray granulation operation, the air outlet temperature is 60-75°C and the atomizer frequency is 80-160Hz.

[0030] In the above-mentioned method for preparing a high-density oxide target, the dispersant in the slurry accounts for 0.1wt% to 5wt% of the slurry weight; the binder accounts for 5wt% to 20wt% of the slurry weight.

[0031] In the above-mentioned method for preparing high-density oxide target materials, the compression molding operation includes compression molding and cold isostatic pressing treatment performed successively. The pressure during compression molding is 85-95Mpa, and the pressure is maintained for 100-140s; the pressure during cold isostatic pressing is 300-400Mpa, and the pressure is maintained for 100-140s.

[0032] In the above-mentioned method for preparing a high-density oxide target, the sintering operation includes a degreasing process and a sintering process;

[0033] The temperature of degreasing treatment is 400℃~600℃;

[0034] After degreasing, sintering is carried out under aerobic conditions, the sintering temperature is 1100-1500°C, the heating rate is 0.1-0.5 / min, and the holding time is 8-12h.

[0035] In addition, the present invention also discloses a high-density oxide target material, which is prepared by any of the above methods.

[0036] This application has at least the following beneficial effects:

[0037] The present invention adjusts the ratio of different particle sizes, adjusts the particle size of large particles and the particle size of small particles, prepares high-density green compacts, and thus improves the density and performance of the target material. DETAILED DESCRIPTION

[0038] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0039] Example 1

[0040] A preparation process of a high-density oxide target is prepared by the following steps:

[0041] Step 1: weigh 99.1 kg of indium oxide, 0.2 kg of cerium oxide, 0.5 kg of titanium oxide, 0.2 kg of tantalum oxide, 8.1 kg of dispersant polyvinyl pyrrolidone and 3.1 kg of binder polyethylene glycol, two portions each, and set aside for later use;

[0042] Step 2: The raw materials weighed in step 1 were dispersed for 30 minutes at a speed of 100 rpm and ground for 4 hours at a speed of 1100 rpm to obtain a slurry with a solid content of 45%. Among them, zirconium balls of 0.3 mm, 0.4-0.6 mm, 0.8-1.0 mm with a weight ratio of 5:3:2 were used for grinding; the volume ratio of zirconium balls to slurry was 0.18;

[0043] Step 3: The slurry obtained in step 2 is sprayed and granulated, and then mixed and sieved to obtain a mixed oxide target precursor powder with an average particle diameter of d. The air outlet temperature is 75°C, the atomizer frequency is 120Hz; d = 20.71nm;

[0044] Step 4: The raw materials weighed in step 1 were dispersed for 30 minutes at a speed of 100 rpm and ground for 4 hours at a speed of 1100 rpm to obtain slurry 2 with a solid content of 45%. Among them, 0.8-1.0 mm zirconium balls were used for grinding; the volume ratio of zirconium balls to slurry was 0.18;

[0045] Step 5: The slurry 2 obtained in step 4 is spray granulated, mixed and sieved to obtain a mixed oxide target precursor powder 2, whose average particle diameter is D. The air outlet temperature is 75°C, the atomizer frequency is 120Hz; D = 50.02nm;

[0046] Step 6: The oxide target precursor powders 1 and 2 are molded and cold isostatically pressed according to the size grading to obtain a target blank containing metal oxide. The pressure during the target molding is 90Mpa, and the pressure is maintained for 120s; the pressure during the cold isostatic pressing is 350Mpa, and the pressure is maintained for 120s. The mass ratio of the oxide target precursor powders 1 and 2 is 80:20;

[0047] Step 7: The obtained pressed embryo is heat treated, the temperature is controlled at 400°C for degreasing treatment (holding time is 5 hours, heating rate is 0.1°C / min), and then cooled to room temperature, oxygen is introduced, and the temperature is increased for sintering to obtain an indium oxide-based target (sintering temperature is 1400°C, heating rate is 0.3°C / min, holding time is 8h), and the density and resistivity of the target are tested.

[0048] Example 2

[0049] A preparation process of a high-density oxide target is basically the same as that of Example 1, except that in step 6, the mass ratio of the oxide target precursor powders one and two is 85:15.

[0050] Example 3

[0051] A preparation process of a high-density oxide target is basically the same as that of Example 1, except that in step 6, the mass ratio of the oxide target precursor powders one and two is 90:10.

[0052] Example 4

[0053] A preparation process of a high-density oxide target is basically the same as that of Example 1, except that the average particle sizes of the oxide target precursor powders 1 and 2 are 23.65 μm and 57.13 μm, respectively.

[0054] Example 5

[0055] A preparation process of a high-density oxide target is basically the same as that of Example 1, except that the average particle sizes of the oxide target precursor powders 1 and 2 are 21.87 μm and 52.83 μm, respectively.

[0056] Example 6

[0057] A preparation process of a high-density oxide target is basically the same as that of Example 1, except that the average particle sizes of the oxide target precursor powders 1 and 2 are 29.41 μm and 71.04 μm, respectively.

[0058] Example 7

[0059] A preparation process of a high-density oxide target is prepared by the following steps:

[0060] Step 1: weigh 97.5 kg of indium oxide, 1 kg of cerium oxide, 1 kg of titanium oxide, 0.5 kg of tantalum oxide, 8.1 kg of dispersant polyvinyl pyrrolidone, and 3.1 kg of binder polyethylene glycol, and set aside in two portions;

[0061] Step 2: The powder, dispersant and additives weighed in step 1 are dispersed for 30 minutes at a rotation speed of 100 rpm and ground for 4 hours at a rotation speed of 1100 rpm to obtain a slurry 1 with a solid content of 45%.

[0062] Among them, zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm with a weight ratio of 5:3:2 were used for grinding; the volume ratio of zirconium balls to slurry was 0.18;

[0063] Step 3: The slurry obtained in step 2 is sprayed and granulated, and then mixed and sieved to obtain a mixed oxide target precursor powder with a particle diameter of d. The air outlet temperature is 75°C, the atomizer frequency is 120Hz; d = 30.51nm;

[0064] Step 4: The powder, dispersant and additives weighed in step 1 are dispersed for 30 minutes at a rotation speed of 100 rpm and ground for 4 hours at a rotation speed of 1100 rpm to obtain slurry 2 with a solid content of 45%.

[0065] Among them, 0.8-1.0 mm zirconium balls are used for grinding; the volume ratio of zirconium balls to slurry is 0.18;

[0066] Step 5: The slurry 2 obtained in step 4 is spray granulated, mixed and sieved to obtain a mixed oxide target precursor powder 2, the particle diameter of which is D. The air outlet temperature is 75°C, the atomizer frequency is 120Hz; D = 73.70nm;

[0067] Step 6: The oxide target precursor powders 1 and 2 are molded and cold isostatically pressed according to the size grading to obtain a target blank containing metal oxide. The pressure during the target molding is 90Mpa, and the pressure is maintained for 120s; the pressure during the cold isostatic pressing is 350Mpa, and the pressure is maintained for 120s. The mass ratio of the oxide target precursor powders 1 and 2 is 80:20;

[0068] Step 7: The obtained pressed embryo is heat treated, the temperature is controlled at 400°C for degreasing treatment (holding time is 5 hours, heating rate is 0.1°C / min), then cooled to room temperature, oxygen is introduced, and the temperature is increased for sintering to obtain an indium oxide-based target (sintering temperature is 1400°C, heating rate is 0.3°C / min, holding time is 8h), and the density and resistivity of the target are tested.

[0069] Example 8

[0070] A preparation process of a high-density oxide target is prepared by the following steps:

[0071] Step 1: weigh 99.7 kg of indium oxide, 0.1 kg of cerium oxide, 0.1 kg of titanium oxide, 0.1 kg of tantalum oxide, 8.1 kg of dispersant polyvinyl pyrrolidone and 3.1 kg of binder polyethylene glycol, two portions each, and set aside for later use;

[0072] Step 2: The powder, dispersant and additives weighed in step 1 are dispersed for 30 minutes at a rotation speed of 100 rpm and ground for 4 hours at a rotation speed of 1100 rpm to obtain a slurry 1 with a solid content of 45%.

[0073] Among them, zirconium balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm with a weight ratio of 5:3:2 were used for grinding; the volume ratio of zirconium balls to slurry was 0.18;

[0074] Step 3: The slurry obtained in step 2 is sprayed and granulated, and then mixed and sieved to obtain a mixed oxide target precursor powder with a particle diameter of d. The air outlet temperature is 75°C, the atomizer frequency is 120Hz; d = 31.58;

[0075] Step 4: The powder, dispersant and additives weighed in step 1 are dispersed for 30 minutes at a rotation speed of 100 rpm and ground for 4 hours at a rotation speed of 1100 rpm to obtain slurry 2 with a solid content of 45%.

[0076] Among them, 0.8-1.0 mm zirconium balls are used for grinding; the volume ratio of zirconium balls to slurry is 0.18;

[0077] Step 5: The slurry 2 obtained in step 4 is spray granulated, mixed and sieved to obtain a mixed oxide target precursor powder 2, the particle diameter of which is D. The air outlet temperature is 75°C, the atomizer frequency is 120Hz; D = 76.28nm;

[0078] Step 6: The oxide target precursor powders 1 and 2 are molded and cold isostatically pressed according to the size grading to obtain a target blank containing metal oxide. The pressure during the target molding is 90Mpa, and the pressure is maintained for 120s; the pressure during the cold isostatic pressing is 350Mpa, and the pressure is maintained for 120s. The mass ratio of the oxide target precursor powders 1 and 2 is 80:20;

[0079] Step 7: The obtained pressed embryo is heat treated, the temperature is controlled at 400°C for degreasing treatment (holding time is 5 hours, heating rate is 0.1°C / min), and then cooled to room temperature, oxygen is introduced, and the temperature is increased for sintering to obtain an indium oxide-based target (sintering temperature is 1400°C, heating rate is 0.3°C / min, holding time is 8h), and the density and resistivity of the target are tested.

[0080] Comparative Example 1

[0081] It is substantially the same as Example 1, except that in step 6, the mass ratio of the oxide target precursor powders 1 and 2 is 50:50.

[0082] Comparative Example 2

[0083] It is substantially the same as Example 1, except that in step 6, the mass ratio of the oxide target precursor powders 1 and 2 is 60:40.

[0084] Comparative Example 3

[0085] It is substantially the same as Example 1, except that in step 6, the mass ratio of the oxide target precursor powders 1 and 2 is 70:30.

[0086] Comparative Example 4

[0087] It is substantially the same as Example 1, except that in step 6, the sizes of the oxide target precursor powders 1 and 2 are both 23-25 ​​μm.

[0088] Comparative Example 5

[0089] It is substantially the same as Example 1, except that in step 6, the sizes of the oxide target precursor powders 1 and 2 are both 56-59 μm.

[0090] Performance Testing

[0091] The test items include relative density and resistivity;

[0092] The test results are shown in Table 1 below;

[0093] Table 1 Test results

[0094]

[0095]

[0096] Result analysis:

[0097] Within the experimental parameter range, the ratio of precursor particles of different sizes is adjusted, and small particles are added to large particles, which effectively solves the problem of large pores and loose particle stacking when large particle powders dominate. The preparation of high-density green bodies also gradually reduces the holes in the target material, and the diameter of the holes is also reduced, so that the compactness of the oxide target material is gradually improved. Comparative Examples 1, 2, and 3 show that the size is not graded according to the set binary particle regular octahedron gap filling and stacking model, resulting in problems such as uneven particle stacking and low density in the green body, which ultimately affects the sintering performance of the target material; Comparative Examples 4 and 5 illustrate the effect of powder particle size grading on the sintering density of the target material. Larger particles form more pores during the sintering process, increasing the porosity; while small particles help to reduce the formation of pores and increase the density of the target material, but too many small particle sizes will affect the filling of particle gaps, resulting in a decrease in density.

[0098] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a high-density oxide target, characterized in that: Mixing the first oxide precursor powder and the second oxide precursor powder, pressing and sintering the mixture to obtain a target material; The first oxide precursor powder and the second oxide precursor powder both contain no less than 97 wt % of indium oxide; The weight of the first oxide precursor powder is equivalent to 80% to 90% of the total weight of the first oxide precursor powder and the second oxide precursor powder; The particle size of the first oxide precursor powder is 20 to 30 μm; the particle size of the second oxide precursor powder is 45 to 73 μm.

2. The method for preparing a high-density oxide target according to claim 1, characterized in that: The first oxide precursor powder and the second oxide precursor powder both contain no less than 98 wt % of indium oxide.

3. The method for preparing a high-density oxide target according to claim 1, characterized in that: The first oxide precursor powder and the second oxide precursor powder further contain one or more combinations of cerium oxide, titanium oxide, tantalum oxide, molybdenum oxide, praseodymium oxide and zinc oxide.

4. The method for preparing a high-density oxide target according to claim 3, characterized in that: The first oxide precursor powder and the second oxide precursor powder contain 97.5wt% to 99.7wt% of indium oxide.

5. The method for preparing a high-density oxide target according to claim 1, characterized in that: The preparation methods of the first oxide precursor powder and the second oxide precursor powder are both: mixing oxide, dispersant and binder to prepare slurry with a solid content of 30wt% to 95wt%, and then sand grinding and spray granulation to obtain powder of corresponding particle size.

6. The method for preparing a high-density oxide target according to claim 5, characterized in that: In the sand milling process of preparing the first oxide precursor powder, the grinding balls used are a mixture of three specifications of grinding balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm; the weight ratio of the grinding balls of 0.3 mm, 0.4-0.6 mm, and 0.8-1.0 mm is 4-7:1-4:1-4; In the sand milling process of preparing the second oxide precursor powder, the grinding balls used are 0.8 mm to 1.0 mm grinding balls.

7. The method for preparing a high-density oxide target according to claim 5, characterized in that: During the sand milling operation, the speed of the sand mill is 800 to 1600 rpm, and the grinding time is 2 to 12 hours; During the spray granulation operation, the air outlet temperature is 60-75°C and the atomizer frequency is 80-160Hz.

8. The method for preparing a high-density oxide target according to claim 5, characterized in that: In the slurry, the dispersant accounts for 0.1wt% to 5wt% of the slurry weight; the binder accounts for 5wt% to 20wt% of the slurry weight.

9. The method for preparing a high-density oxide target according to any one of claims 1 to 8, characterized in that: The compression molding operation includes compression molding and cold isostatic pressing, the pressure during compression molding is 85-95 MPa, and the pressure is maintained for 100-140 seconds; the pressure during cold isostatic pressing is 300-400 MPa, and the pressure is maintained for 100-140 seconds; The sintering operation includes a degreasing process and a sintering process; The temperature of degreasing treatment is 400℃~600℃; After degreasing, sintering is carried out under aerobic conditions, the sintering temperature is 1100-1500°C, the heating rate is 0.1-0.5 / min, and the holding time is 8-12h.

10. A high-density oxide target, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of indium tin oxide evaporation target material

    CN113185279A

  • Low-zirconium-content indium cerium tantalum titanium oxide target material and preparation method thereof

    CN116835964A

  • Tungsten indium oxide target material and preparation method thereof

    CN118307297A

  • Preparation method of high density ITO target through low temperature sintering process and ITO target prepared thereby