Preparation method and application of Janus fractal network material for in-situ growth of double MOFs
By growing CuTCNQ and CuBTC MOF in situ on leaf veins to form an asymmetric microstructure Janus fractal network, the problem of droplet transport in a timely manner was solved, achieving efficient mist collection, simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202410941933.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-15
AI Technical Summary
When existing technologies mimic leaf vein structure for mist collection, the droplets cannot be transported in time after spreading into a water film on the leaf veins, resulting in reduced collection efficiency. Furthermore, the process is complex and requires additional low surface energy materials for modification.
By growing hydrophobic CuTCNQ and hydrophilic CuBTC MOF in situ on opposite sides of metal leaf veins, an asymmetric Janus fractal network is formed. The directional transport of droplets is achieved by utilizing the Laplace pressure difference and capillary force, simplifying the process and eliminating the need for additional low surface energy material modification.
The process improved the mist collection efficiency to 1.23 g/cm²/h, which is 292.9% higher than that of the original bare leaf veins. The process is simple, low-cost, and the materials are non-toxic and harmless.
Smart Images

Figure CN118932322A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adjustable wettability of material surfaces and interfaces, and in particular to a preparation method and application of a Janus fractal network material of in-situ grown dual MOFs. Background Art
[0002] Nature always gives humans a variety of optimized and effective fractal network structures, such as blood vessels, rivers, branches, leaf veins, etc. These complex fractal network structures have perfect self-similarity. Among them, the fractal network structure inspired by leaf veins has become one of the most classic and successful bionic prototypes, and has great application potential in many fields. Leaf veins are known as the "blood vessels" and "skeletons" on plant leaves, responsible for capturing sunlight and transporting water efficiently with the lowest energy consumption. Many researchers have collected fog water by imitating the structure of leaf veins, but most of them are based on 3D printing technology to imitate the macroscopic appearance of leaf veins, and do not use real leaf vein structures. Although the fractal network structure of leaf veins helps the directional transmission of droplets. However, when the collected droplets spread into a water film on the leaf veins, the droplets cannot be transported away in time, and a fresh surface cannot be generated, resulting in a significant reduction in its fog water collection efficiency. Summary of the invention
[0003] The present invention provides a preparation method and application of a Janus fractal network material of in-situ grown dual MOFs. A Janus fractal metal network with an asymmetric microstructure and a wettability gradient is obtained by in-situ growing two different MOFs (hydrophobic CuTCNQ and hydrophilic CuBTC) on opposite sides (front and back) of metallized leaf veins. The CuTCNQ nanoneedles are in the shape of cactus thorns. Once the mist water nucleates and grows on the top of the CuTCNQ microneedles, the condensed tiny droplets will penetrate from the hydrophobic side of the leaf vein network to the hydrophilic side under the action of the Laplace pressure difference and capillary force, and refresh the dry hydrophobic surface to carry out a new round of mist collection. Compared with the traditional bare leaf vein structure for mist water collection, it solves the problem that when the collected droplets spread into a water film on the leaf veins, the droplets cannot be transported in time and the fresh surface cannot be generated, thereby greatly reducing the collection efficiency. Moreover, the method provided by the present invention further shortens the process flow, prepares a super-hydrophobic structure in one step, does not require additional low-surface energy materials for modification, achieves fluorination-free treatment, and provides a design idea for the development of efficient and green fog water collectors.
[0004] The present invention solves the above technical problems as follows: A method for preparing a Janus fractal network material of in-situ grown dual MOFs comprises the following steps:
[0005] 1) remove the leaf pulp and wash it to obtain the leaf veins;
[0006] The specific operation is as follows: After cleaning the leaves, soak them in a mixed aqueous solution of sodium hydroxide and sodium carbonate, heat and boil for 15 to 20 minutes, and gently brush off the leaf flesh with a soft brush, leaving intact leaf veins. Then, put the leaf veins into deionized water to remove the residual leaf flesh by ultrasonic, and then put them into a 10% H2O2 aqueous solution for bleaching for 20 to 30 minutes, and rinse them with deionized water to obtain the leaf veins. The leaves are preferably white magnolia leaves.
[0007] 2) Place the leaf veins in a medium containing Sn 2+ Soak in the sensitizing solution for 5 to 10 minutes, rinse with deionized water, and then place in the Ag-containing + After soaking in the activation solution for 5 to 10 minutes and in the formaldehyde solution for 5 to 10 seconds, the leaf veins with Ag nanoparticles deposited on the surface were obtained after being washed with deionized water;
[0008] 3) immersing the leaf veins with Ag nanoparticles deposited on the surface in an electrolyte solution containing copper sulfate for electroplating, washing with deionized water and then drying to obtain copper-plated leaf veins;
[0009] 4) placing the copper-plated leaf vein above the steam formed by heating the 7,7,8,8-tetracyanobenzoquinodimethane / acetonitrile solution, so that the 7,7,8,8-tetracyanobenzoquinodimethane is deposited on one side of the copper-plated leaf vein to form a super-hydrophobic CuTCNQ film;
[0010] The specific operation is as follows: Use high-temperature tape to fix the copper-plated leaf vein on the top of the glass culture dish, and then take an appropriate amount of TCNQ / acetonitrile solution and place it at the bottom of the glass culture dish. Place the glass culture dish on a heating table and heat it. Under instantaneous heating, a large amount of TCNQ vapor will be generated to react with the Cu on the top of the glass culture dish to form CuTCNQ. Finally, a layer of black-purple film is deposited on the front side of the copper-plated leaf vein (the back side of the copper-plated leaf vein fits tightly with the glass culture dish, and the front side of the copper-plated leaf vein faces downward to react with TCNQ vapor), indicating that CuTCNQ nanoneedles have successfully grown on the surface of the copper-plated leaf vein.
[0011] 5) Then the other side of the copper-plated leaf vein is floated on the hydrophilic solution. After the reaction is completed, a hydrophilic CuBTC film is formed on the other side of the copper-plated leaf vein. After washing and drying, a Janus fractal network water-collecting material is obtained.
[0012] The purpose of this application is to process the leaves into veins and place them in the sensitizing solution to make the vein surface full of Sn 2+ ions, after being activated by the activation solution, Ag + ions are reduced to Ag nanoparticles and deposited on the surface of leaf veins, while Sn 2+ The ions are oxidized to Sn 4+ The reaction during the activation process is shown below:
[0013] 2Ag+ +Sn 2+ =2Ag+Sn 4+
[0014] After the leaf veins are copper-plated, hydrophobic / hydrophilic MOFs can be grown in situ on the surface of the leaf veins, and the structural characteristics of the leaf veins can be used to achieve directional transport of droplets. One side (front) of the copper-plated leaf veins reacts with TCNQ hot vapor to generate super-hydrophobic CuTCNQ nanoneedles, while the other side (back) remains floating on the target solution to react and generate hydrophilic CuBTC, forming a Janus fractal metal network with asymmetric microstructure and wettability differences. The CuTCNQ nanoneedles are morphologically very similar to the cactus cone thorns used for fog water collection. This thorn structure can intercept micron-sized water droplets in the fog and transfer the droplets to the other side - CuBTC through Laplace pressure difference. CuBTC is considered to be an ideal adsorbent for water collection in a variety of environments (dry-humid-fog), and its rod-like structure is widely used in the field of atmospheric water collection. As a hydrophilic MOF, CuBTC can not only quickly collect micron-sized droplets, but also accelerate the transmission of collected droplets.
[0015] Preferably, in step 2), Sn 2+ Sn in sensitizing solution 2+ The concentration is 0.12~0.14mol / L.
[0016] The Sn-containing 2+ The preparation steps of the sensitizing solution are as follows: 4 ml of 98% concentrated sulfuric acid, 3 g of stannous chloride dihydrate, and 30-40 mg of tin particles are put into 100 ml of deionized water to obtain the sensitizing solution.
[0017] Preferably, in step 2), Ag is contained + Ag in activation solution + The concentration is 0.01~0.03mol / L.
[0018] The preparation steps of the activation solution are as follows: 0.3-0.5 g of silver nitrate is added into 100 ml of deionized water, and ammonia water is added dropwise until the solution becomes clear to obtain the activation solution.
[0019] Preferably, in step 3), the electrolyte solution contains Cu 2+ The concentration is 0.03~0.05mol / L.
[0020] The preparation method of the electrolyte solution is as follows: 5g of copper sulfate pentahydrate, 20g of potassium sodium tartrate, 10g of disodium ethylenediaminetetraacetate, 2g of nickel chloride, and 4g of sodium hydroxide are added to 500ml of deionized water to prepare an electrolyte solution. The electrolysis steps are as follows: the leaf vein is connected to the negative electrode of the power supply, the graphite sheet is connected to the positive electrode of the power supply, the leaf vein is electroplated in the copper-containing electrolyte solution for 20 to 30 minutes, and the leaf vein is taken out and rinsed with deionized water.
[0021] Preferably, in step 4), the concentration of the 7,7,8,8-tetracyanobenzoquinodimethane / acetonitrile solution is 1 mol / L.
[0022] Preferably, in step 4), the heating temperature is 170-220° C. and the heating time is 40-80 min.
[0023] Preferably, in step 5), the hydrophilic solution is a mixed water / ethanol solution of copper nitrate of trimesic acid.
[0024] Preferably, in the hydrophilic solution, the concentration of trimesic acid is 2.1 g / L, the concentration of copper nitrate is 3.4 g / L; and the volume ratio of ethanol to water is 1:7.
[0025] The mixed solution with this concentration ratio can keep the leaf veins floating on the surface of the solution and does not come into contact with the CuTCNQ superhydrophobic film on the front side of the leaf veins.
[0026] Preferably, in step 5), the reaction time is 90 to 120 minutes.
[0027] The application of an in-situ grown dual MOF Janus fractal network material prepared by the method described above in the preparation of a fog water collector.
[0028] The beneficial effects of the present invention are:
[0029] 1. The process provided by the present invention is simple, the raw materials are easily available, the cost is low, and it is non-toxic and harmless;
[0030] 2. The prepared dual-MOF Janus fractal network material has significant wettability differences. The contact angle on the CuTCNQ side can reach 156.5°, the rolling angle is less than 2°, and the contact angle on the CuBTC side can reach 67.5°.
[0031] 3. The prepared dual-MOF Janus fractal network material has high fog water collection efficiency, and its fog water collection efficiency value reaches 1.23g / cm 2 / h, compared to 0.42g / cm 2 / h, the fog water collection efficiency increased by 292.9%.
[0032] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0034] Figure 1 The flow chart for the preparation of Janus fractal network water-collecting materials;
[0035] Figure 2 The scanning electron microscope image, contact angle and EDS spectrum of the Janus fractal network water-collecting material and its intermediate product prepared in Example 1:
[0036] (a) is a scanning electron microscope image of the copper-plated leaf vein surface and its static water contact angle after completing step 1;
[0037] (b) is a scanning electron microscope image of the superhydrophobic CuTCNQ leaf vein surface and its static water contact angle after completing step 2;
[0038] (c) is a scanning electron microscope image of the hydrophilic CuBTC leaf vein surface and its static water contact angle after completing step 3;
[0039] (d) is the scanning electron microscope image of the longitudinal section of the Janus fractal network water-collecting material and its static contact angle;
[0040] (e) EDS spectra of Cu, C, and N elements on the surface of CuTCNQ leaf veins with superhydrophobic MOF;
[0041] (f) EDS spectra of Cu, C, and O elements on the surface of CuBTC veins with hydrophilic MOF;
[0042] (g) is the rolling contact angle of the CuTCNQ leaf vein surface with superhydrophobic MOF;
[0043] (h) is a photo of the hydrophilic side of a water droplet falling on the prepared Janus quasi-fractal network of the dual MOF;
[0044] Figure 3 Infrared, UV-Vis, Raman, XPS, XRD spectra and TEM images of the dual-MOF Janus fractal network water-collecting material prepared in Example 1:
[0045] (a) IR spectra of CuTCNQ and CuBTC on the Janus fractal network surface of dual MOF;
[0046] (b) UV absorption spectra of CuTCNQ and CuBTC on the Janus fractal network surface of dual MOF;
[0047] (c) Raman spectra of CuTCNQ and CuBTC on the Janus fractal network surface of the dual MOF;
[0048] (d) Fine spectra of Cu 2p of CuTCNQ and CuBTC on the Janus fractal network surface of the dual MOF;
[0049] (e) XRD spectra of CuTCNQ and CuBTC on the Janus fractal network surface of dual MOF;
[0050] (f) TEM image of CuTCNQ on the Janus fractal network surface of the dual MOF.
[0051] Figure 4 These are optical photographs corresponding to samples at different stages in the preparation process of Example 1 of the present invention: a is the exposed leaf vein after removing the leaf flesh; b is the copper-plated leaf vein; c is the CuTCNQ leaf vein with superhydrophobic MOF.
[0052] Figure 5 a is a diagram of the experimental device for collecting fog water; b is the fog water collection efficiency corresponding to the original bare leaf veins (LV) in Example 1 of the present invention, the CuTCNQ leaf veins (CT-LV) in Example 1, the CuBTC leaf veins (CB-LV) in Comparative Example 1, and the Janus leaf veins (J-LV) with dual MOFs in Example 1; c is a photograph of the droplet behavior changing with time on the surface of the original bare leaf veins (LV) in Example 1 of the present invention, the CuTCNQ leaf veins (CT-LV) in Example 1, the CuBTC leaf veins (CB-LV) in Comparative Example 1, and the Janus leaf veins (J-LV) with dual MOFs in Example 1 during the fog water collection process. DETAILED DESCRIPTION
[0053] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0054] Example 1
[0055] like Figure 1 As shown, this embodiment provides a method for preparing a Janus fractal network water-collecting material, and the steps are as follows:
[0056] 1) Remove the mesophyll from the leaves
[0057] This embodiment uses natural magnolia leaves, and the main veins are thick and the vein density is large, the leaves are beautiful in shape and of appropriate size. The selected magnolia leaves are cleaned and soaked in 300ml deionized water containing 10.5g sodium hydroxide and 6g sodium carbonate, and heated and boiled for 15-20min. After taking out, wash, and then use a soft brush to gently brush off the leaf flesh, leaving intact leaf veins. Then put the leaf veins into deionized water, and use ultrasound to remove the residual leaf flesh on the leaf veins. Afterwards, put the leaf veins into a 10% H2O2 aqueous solution for bleaching for 20-30min, and then rinse thoroughly with deionized water.
[0058] 2) Preparation of leaf veins with Ag nanoparticles deposited on the surface
[0059] a. Put 4 ml of 98% concentrated sulfuric acid, 3 g of stannous chloride dihydrate, and 30-40 mg of tin particles (two particles) into 100 ml of deionized water to prepare Sn-containing 2+ Sensitization solution. Soak the leaf veins in the sensitization solution for 5 to 10 minutes, then rinse with deionized water. In this step, the purpose of sensitization is to fill the surface of the leaf veins with Sn. 2+ ions, paving the way for the next step of activation.
[0060] b. Add 0.4g silver nitrate to 100ml deionized water, add ammonia water until the solution becomes clear, and prepare Ag-containing + Activation solution. Soak the leaf veins treated with the previous step in the activation solution for 5 to 10 minutes. Then soak them in a 10% formaldehyde solution for 5 to 10 seconds, and finally rinse them with deionized water. In this step, Ag + ions are reduced to Ag nanoparticles and deposited on the surface of leaf veins, while Sn 2+ The ions are oxidized to Sn 4+ Ag nanoparticles are the core of leaf vein chemical copper plating. The reaction during the activation process is shown in the following formula:
[0061] 2Ag + +Sn 2+ =2Ag+Sn 4+
[0062] 3) Electroplating leaf veins
[0063] Connect the leaf veins to the negative pole of the power supply, the graphite sheet to the positive pole of the power supply, and put 5g of copper sulfate pentahydrate, 20g of potassium sodium tartrate, 10g of disodium ethylenediaminetetraacetate, 2g of nickel chloride, and 4g of sodium hydroxide into 500ml of deionized water to prepare an electrolyte solution. In order to make the leaf veins more conductive during electroplating, a circle of conductive copper glue needs to be wrapped around the petiole. In addition, in order to make the copper plated on the leaf veins uniform and dense, the current needs to be set to 0.1A. Electroplate the leaf veins in the copper electroplating solution for 20 to 30 minutes, remove the leaf veins and rinse them with deionized water.
[0064] 4) In situ growth of superhydrophobic MOF-CuTCNQ on copper-plated leaf veins
[0065] The copper-plated veins were washed with hydrochloric acid, deionized water, acetone, and ethanol in turn, and then dried with nitrogen (the washed and dried veins should react immediately to minimize the oxidation time, otherwise a layer of CuO will be generated on the surface of the copper-plated veins, which will affect the next step of the reaction). The copper-plated veins were pasted on the upper surface of the inner surface of the glass culture dish with high-temperature tape, and then 5 to 10 ml of 1M TCNQ / acetonitrile solution was placed on the bottom of the glass culture dish, and finally heated at 220°C for 40 minutes to deposit TCNQ on the upper surface of the copper-plated veins (the back of the copper-plated veins fit tightly with the glass culture dish, and the front of the copper-plated veins faced downward to react with TCNQ vapor) to form a CuTCNQ film, and a CuTCNQ vein with a superhydrophobic MOF was obtained.
[0066] 5) In situ growth of hydrophilic MOF-CuBTC on copper-plated leaf veins
[0067] 0.168g BTC was dissolved in 10ml anhydrous ethanol to prepare solution A, and 0.35g copper nitrate trihydrate was dissolved in 70ml deionized water to prepare solution B. Then solution A and solution B were mixed to prepare solution C, and the CuTCNQ leaf veins from the previous step were floated on solution C and reacted at room temperature for 120min. When the CuTCNQ leaf veins were placed on solution C, the leaf veins were gently compacted with tweezers so that the back of the leaf veins were fully in contact with solution C for reaction, while the front of the leaf veins were fully exposed to the air. After the reaction was completed, the back of the leaf veins was contacted with deionized water and floated in deionized water, and gently shaken with tweezers to remove the unreacted substances remaining on the surface, and then placed in an oven at 60°C for 5 to 10min. Finally, a Janus fractal network water-collecting material with dual MOFs with asymmetric microstructure and different wettability was obtained.
[0068] Comparative Example 1
[0069] This comparative example provides a CuBTC leaf vein with a super-hydrophilic MOF on its surface. The preparation steps are exactly the same as steps 1-3 of Example 1, except that after the leaf vein is copper-plated, the copper-plated leaf vein is directly immersed in the mixed solution C described in step 5 of Example 1 and reacted at room temperature for 4 hours to obtain a leaf vein with a hydrophilic CuBTC film.
[0070] The morphology analysis of Example 1 and its intermediate product was performed, and the results were as follows: Figure 2 As shown. It can be found that after the copper-plated leaf veins react with the TCNQ / acetonitrile solution, fluffy needle-like structures will grow on the surface ( Figure 2b), in the enlarged image, it can be seen that this structure is composed of disordered nanoneedles, which increases the surface roughness and makes its surface static contact angle reach 156.5°. At this time, the leaf veins can float stably on the water surface. By adjusting the ratio of anhydrous ethanol and deionized water in solution C, the CuTCNQ leaf veins can be floated on solution C so that the back of the leaf veins reacts with BTC to generate hydrophilic CuBTC, and its hydrophilic surface static contact angle reaches 67.5° ( Figure 2 c). The front side of the leaf veins exposed to air does not react with solution C and still maintains the superhydrophobicity of CuTCNQ. Finally, a Janus quasi-fractal metal network of dual MOFs with asymmetric microstructure and different wettability can be obtained. Figure 2 d shows that the upper surface of the leaf vein is a super-hydrophobic surface, and the lower surface is a hydrophilic surface. Figure h shows the difference in wettability of the Janus quasi-fractal network of the dual MOF prepared in Example 1. When a water drop falls on its hydrophilic surface and uses it as the lower surface and places it parallel to the ground, the drop still cannot fall under the action of its gravity. At this time, the upper surface is the super-hydrophobic surface side, and the water drop cannot stay on it and rolls down directly. Figure 2 e and f are the EDS spectra of the corresponding elements of CuTCNQ and CuBTC, respectively, which indicate the successful in situ growth of CuTCNQ and CuBTC.
[0071] like Figure 3 As shown, infrared, UV-Vis, Raman, XPS, XRD characterization tests and TEM images further proved that CuTCNQ and CuBTC successfully grew on the surface of leaf veins.
[0072] like Figure 4 As shown, Figures ac are optical photographs of leaf veins corresponding to different operation steps in Example 1, which are bare leaf veins, copper-plated leaf veins and CuTCNQ leaf veins respectively.
[0073] like Figure 5 As shown, in a closed space, the relative humidity is controlled at about 90%, and the mist flow speed is set to 0.4-0.5 m / s. Figure c shows the nucleation, accumulation, and directional transportation of droplets on the surface of the original leaf veins in Example 1, the CuTCNQ leaf veins in Example 1, the CuBTC leaf veins in Comparative Example 1, and the Janus leaf veins with dual MOF in Example 1. After a mist collection test with 3 cycles per group every 15 minutes, the mist collection efficiency of the Janus leaf vein surface with dual MOF reached 1.23 g / cm 2 / h, compared to 0.42g / cm 2 / h, the fog water collection efficiency increased by 292.9%.
[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a Janus fractal network material with in-situ growth of dual MOFs, It is characterized in that The following steps are involved: 1) remove the leaf pulp and wash it to obtain the leaf veins; 2) Place the leaf veins in a medium containing Sn 2+ Soak in sensitizing solution, rinse with deionized water, and then place in Ag-containing + After soaking in activation solution and formaldehyde solution and washing with deionized water, leaf veins with Ag nanoparticles deposited on the surface were obtained; 3) immersing the leaf veins with Ag nanoparticles deposited on the surface in an electrolyte solution containing copper sulfate for electroplating, washing with deionized water and then drying to obtain copper-plated leaf veins; 4) placing the copper-plated leaf vein above the steam formed by heating the 7,7,8,8-tetracyanobenzoquinodimethane / acetonitrile solution, so that the 7,7,8,8-tetracyanobenzoquinodimethane is deposited on one side of the copper-plated leaf vein to form a super-hydrophobic CuTCNQ film; 5) Then the other side of the copper-plated leaf vein is floated on the hydrophilic solution. After the reaction is completed, a hydrophilic CuBTC film is formed on the other side of the copper-plated leaf vein. After washing and drying, a Janus fractal network water-collecting material is obtained.
2. A method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In step 2), Sn 2+ Sn in sensitizing solution 2+ The concentration is 0.12~0.14mol / L.
3. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In step 2), Ag + Ag in activation solution + The concentration is 0.01~0.03mol / L.
4. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In step 3), Cu in the electrolyte solution 2+ The concentration is 0.03~0.05mol / L.
5. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In the step 4), the concentration of the 7,7,8,8-tetracyanobenzoquinodimethane / acetonitrile solution is 1 mol / L.
6. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In the step 4), the heating temperature of the 7,7,8,8-tetracyanobenzoquinodimethane / acetonitrile solution is 170-220° C. and the heating time is 40-80 minutes.
7. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In the step 5), the hydrophilic solution is a mixed water / ethanol solution of trimesic acid / copper nitrate.
8. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 7, It is characterized in that In the hydrophilic solution, the concentration of trimesic acid is 2.1 g / L, the concentration of copper nitrate is 3.4 g / L; and the volume ratio of ethanol to water is 1:
7.
9. The method for preparing a Janus fractal network material of in-situ grown dual MOF according to claim 1, It is characterized in that In the step 5), the reaction time is 90 to 120 minutes.
10. Use of the Janus fractal network material prepared by the method of claims 1-9 in fog water collection.
Citation Information
Patent Citations
Self-driven water collecting surface with super-hydrophobic-super-hydrophilic structure and preparation method thereof
CN108816702A
CuTCNQ@CuBTC core-shell material and preparation method thereof
CN112225914A
CuBTC nano pesticide preparation for controlling pine wood nematodes and vector insect monochamus alternatus of pine wood nematodes
CN115474614A
Ni-MOF thin-film photocatalyst grown in-situ on foamed nickel surface, preparation method therefor, and use thereof
WO2022041852A1