Preparation method of composite diaphragm for hydrogen production by water electrolysis and product thereof

By modifying the zirconia powder and combining it with polymer resin, composite membranes are prepared, and the swelling and corrosion problems of alkaline electrolytic cell membranes under high current load and high temperature are solved, and excellent hydrophilic and mechanical properties are achieved, and the company has extended the Lifespan and stability are improved.

CN118932411APending Publication Date: 2024-11-12ZHEJIANG NHU SPECIAL MATERIALS CO LTD +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411010288.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing alkaline electrolytic cell membranes have swelling and corrosion problems under high current load and high temperature environments, resulting in a shortened service life and the problem of falling off of hydrophilic inorganic particles is difficult to completely solve.

Method used

By modifying the zirconia powder, combining polymer resin with polyphenylene sulfide mesh to convert it, a composite separator with excellent hydrophilic properties, mechanical properties and alkali stability is prepared, and zirconia and polyphenylene sulfide are improved. adhesion force.

Benefits of technology

It significantly improves the adhesion of the composite diaphragm, extends its service life, ensures stability and tensile strength in high temperature and high alkali environments, and has low surface resistance, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964135340000111
    Figure BDA0004964135340000111
  • Figure BDA0004964135340000121
    Figure BDA0004964135340000121
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite diaphragm for hydrogen production by electrolysis of water, which comprises the following steps: 1) mixing zirconium oxide powder with an alkaline solution, and heating and modifying to obtain modified zirconium oxide; the specific surface area of the zirconium oxide powder is 10-50m < 2 > / g, and the average particle size D50 is 0.5-3.0 mu m; the surface hydroxyl density of the modified zirconium oxide obtained after heating modification is (1-6) nOH / nm < 2 >; 2) mixing polymer resin, modified zirconium oxide and an organic solvent, and uniformly stirring to obtain slurry; and 3) coating two sides of a polyphenylene sulfide net with the slurry, and carrying out phase conversion to obtain the composite diaphragm for hydrogen production by electrolysis of water. The preparation method disclosed by the invention is simple in process, controllable and easy to implement; the prepared composite diaphragm is excellent in hydrophilic performance and mechanical property, low in surface resistance and excellent in alkali liquor stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diaphragms, and in particular to a preparation method of a composite diaphragm for producing hydrogen by electrolyzing water and a product thereof. Background Art

[0002] Hydrogen energy, as an efficient and clean secondary energy source, has attracted widespread attention from all over the world. Large-scale and low-cost production of H2 is one of the important links in the development and utilization of H2 energy. Hydrogen production by water electrolysis has the advantages of relatively simple operation, relatively mature technology, high purity of produced H2, and no pollution in the hydrogen production process. It is an important means to achieve large-scale production of H2. At present, domestic alkaline water electrolysis dominates the water electrolysis industry.

[0003] Usually, an electrolyte (usually 20-40wt% potassium hydroxide aqueous solution) is filled into an alkaline electrolytic cell, and water is decomposed under the action of direct current, producing H2 at the cathode and O2 at the anode. The diaphragm strictly isolates the produced H2 and O2, while allowing the free movement of OH- ions in the circuit of the electrolytic cell. The quality of the diaphragm is directly related to the purity and power consumption of H2 and O2, so it has become a hot topic of research. The requirements for the diaphragm include:

[0004] 1) It can be wetted by the electrolyte, so that the ions in the solution can pass smoothly;

[0005] 2) Good air tightness, which does not affect the safe operation of the electrolyzer and the purity of the outlet gas;

[0006] 3) Have sufficient mechanical strength;

[0007] 4) It is not corroded by alkali solution in the electrolyte and has strong chemical stability;

[0008] 5) Cheap and suitable for industrial use.

[0009] For a long time, the main raw material of alkaline electrolytic cell diaphragms has been asbestos. Asbestos diaphragms have good hydrophilic properties and easy ion permeability. However, the swelling and chemical instability of asbestos diaphragms themselves cause them to have serious swelling defects in specific operating environments, especially under high current loads, resulting in a shortened service life. Moreover, due to the limitations of the asbestos material itself, the electrolyte temperature can only be controlled below 90°C. When the electrolyte temperature exceeds 90°C, the corrosion of the asbestos diaphragm intensifies, thereby polluting the electrolyte and affecting its service life. For the above reasons, the development of new diaphragm materials that can replace asbestos diaphragms has become an important topic in the industry.

[0010] Polyphenylene sulfide (PPS) has the advantages of stable chemical properties, high temperature resistance, and resistance to harsh water electrolysis conditions such as concentrated alkali, making it a popular choice to replace asbestos diaphragms. However, PPS is highly hydrophobic and needs to be treated by grafting, oxidation, sulfonation, plasma, etc. to form a hydrophilic surface.

[0011] For example, a Chinese patent document with application publication number CN 110869538 A discloses a reinforced diaphragm for alkaline hydrolysis, which comprises a porous support, a first porous polymer layer adjacent to one side of the support, and a second porous polymer layer adjacent to the other side of the support, wherein the maximum pore sizes of the porous polymer layers on both sides of the support are different from each other and the ratio of the two is between 1.25 and 10; the first and second porous polymer layers both comprise a membrane polymer and a hydrophilic inorganic material. When the reinforced diaphragm is used in an electrolytic cell, during the use of the electrolytic cell, the alkali solution will flow on the surface of the diaphragm, and in addition, due to the unstable electric energy, a pressure difference will be generated on both sides of the diaphragm, both of which will cause the diaphragm to vibrate for a long time, resulting in the shedding of hydrophilic inorganic particles.

[0012] Another example is a Chinese patent document with application publication number CN 107250437 A, which discloses a diaphragm for alkaline water electrolysis, an alkaline water electrolysis device, a method for manufacturing hydrogen, and a method for manufacturing a diaphragm for alkaline water electrolysis. The diaphragm for alkaline water electrolysis has a polymer porous membrane containing a polymer resin and hydrophilic inorganic particles, the porosity of the polymer porous membrane is 30-60%, the average pore size of the two surfaces of the polymer porous membrane is 0.5-2.0 μm, and the ratio of the mode particle size of the hydrophilic inorganic particles to the average pore size of the polymer porous membrane is more than 2.0. Although this technical solution alleviates the problem of falling off of hydrophilic inorganic particles to a certain extent, due to the physical bond between the hydrophilic inorganic particles and the high molecular polymer, the bonding strength is low, and the falling off problem cannot be fundamentally solved, especially in a long-term and harsh environment. In addition, it is not easy to control the average pore size of the surface by phase inversion method. Summary of the invention

[0013] In view of the deficiencies in the prior art, the present invention discloses a method for preparing a composite diaphragm for producing hydrogen by electrolyzing water. The prepared composite diaphragm has excellent hydrophilicity, mechanical properties, low surface resistance, and excellent alkaline solution stability.

[0014] The specific technical solutions are as follows:

[0015] A method for preparing a composite diaphragm for producing hydrogen by electrolysis of water comprises the following steps:

[0016] 1) mixing zirconium oxide powder with an alkaline solution, and heating and modifying the mixture to obtain modified zirconium oxide;

[0017] The specific surface area of ​​the zirconium oxide powder is 10 to 50 m2 / g, average particle size D50 is 0.5~3.0μm;

[0018] The surface hydroxyl density of the modified zirconium oxide obtained after heating modification is (1-6) nOH / nm 2 ;

[0019] 2) mixing the polymer resin, modified zirconium oxide and an organic solvent, and stirring them evenly to obtain a slurry;

[0020] 3) coating the slurry on both sides of the polyphenylene sulfide network, and obtaining the composite diaphragm for producing hydrogen by electrolysis of water after phase conversion.

[0021] The preparation method disclosed in the present invention is to modify zirconium oxide, prepare slurry and coat it on both sides of the polyphenylene sulfide net, and prepare a composite diaphragm after phase conversion. The method can significantly improve the bonding force between zirconium oxide and polyphenylene sulfide, on the one hand, solve the problem of shedding after long-term operation caused by directly blending zirconium oxide and polyphenylene sulfide in the prior art, and on the other hand, prepare a composite diaphragm with excellent hydrophilicity, mechanical properties, low surface resistance, and excellent alkali solution stability. The key to the preparation method is to screen the specific surface area and average particle size of zirconium oxide within a suitable range, and further control the surface hydroxyl density of the modified zirconium oxide obtained after modification.

[0022] The specific surface area of ​​the zirconium oxide powder can be specifically 10 m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g, 30m 2 / g, 35m 2 / g, 40m 2 / g, 45m 2 / g, 50m 2 / g or any value in the range.

[0023] The average particle size D50 of the zirconium oxide powder may be 0.5 μm, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm or any value within the range.

[0024] The surface hydroxyl density of the modified zirconium oxide obtained after heating modification can be specifically 1.0nOH / nm 2 、1.5nOH / nm 2 , 2.0nOH / nm 2 、2.5nOH / nm 2 、3.0nOH / nm 2 、3.5nOH / nm 2 、4.0nOH / nm 2 、4.5nOH / nm2 、5.0nOH / nm 2 、5.5nOH / nm 2 、6.0nOH / nm 2 Or any value in the range.

[0025] The test found that only when the specific surface area is 10 to 50 m 2 / g, the average particle size D50 of zirconium oxide is 0.5-3.0 μm; and the surface hydroxyl density of the modified zirconium oxide is controlled at (1-6) nOH / nm 2 Only in this way can the above-mentioned invention objectives be achieved.

[0026] In step 1):

[0027] After being treated with an alkaline solution, -OH groups can be chemically grafted on the surface of zirconium oxide. The present invention has no special requirements on the type of the alkaline solution, and it can be selected from conventional types in the art, such as sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, sodium bicarbonate aqueous solution, etc.

[0028] There is no special requirement for the concentration of the alkaline solution, which can be 5-50wt%. When the concentration of the alkaline solution is high, the temperature of the heating modification can be appropriately lowered, and the time of the heating modification can be appropriately shortened. When the concentration of the alkaline solution is low, the temperature and time of the heating modification are adjusted in the opposite way to the above description, as long as the surface hydroxyl density of the modified zirconium oxide after modification is ensured to be (1-6) nOH / nm 2 Within the range.

[0029] The surface hydroxyl density in the present invention refers to the number of moles of hydroxyl groups per square nanometer.

[0030] There is no special requirement for the amount of the alkaline solution, which only needs to be enough to immerse the zirconium oxide powder.

[0031] Preferred:

[0032] The heating modification temperature is 60-100°C, specifically 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C or any value within the range.

[0033] The time for heating modification is 1 to 24 hours, specifically 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours or any value within the range.

[0034] In step 2):

[0035] The polymer resin is selected from one or more of polysulfone, polyethersulfone and polyphenylsulfone;

[0036] Preferably, it is a polysulfone resin having a weight average molecular weight of 30,000 to 100,000 and a distribution index of 3 to 4.

[0037] The organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N-ethyl-pyrrolidone, acetonitrile and dimethyl sulfoxide.

[0038] Preferred:

[0039] The mass ratio of polymer resin to modified zirconia is 1:(1.5-9.0), specifically 1:1.5, 1:2.0, 1:2.5, 1:3.0, 1:3.5, 1:4.0, 1:4.5, 1:5.0, 1:5.5, 1:6.0, 1:6.5, 1:7.0, 1:7.5, 1:8.0, 1:8.5, 1:9.0 or any ratio within the range.

[0040] The mass volume ratio of the polymer resin to the organic solvent is 1:(1-30) g / mL, and can be specifically 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:20, 1:25, 1:30 or any ratio within the range.

[0041] Preferred:

[0042] In step 2), all raw materials are stirred evenly under vacuum conditions to obtain slurry. It is found through experiments that the composite diaphragm prepared by stirring the slurry under vacuum conditions and then coating has higher tensile strength and better stability.

[0043] It is further preferred that the absolute pressure is controlled to be ≤10 kPa, and specifically may be 0.01 kPa, 0.1 kPa, 1 kPa, 2 kPa, 3 kPa, 4 kPa, 5 kPa, 6 kPa, 7 kPa, 8 kPa, 9 kPa, 10 kPa or any value within the range.

[0044] In step 3):

[0045] The phase inversion process can make the organic solvent quickly enter the water phase, causing the polymer resin to precipitate and solidify from the slurry to form a porous membrane.

[0046] The phase transformation is specifically:

[0047] The coated polyphenylene sulfide mesh was placed in air for pre-evaporation and then placed in a water bath for standing.

[0048] The air humidity is (50-90) RH%, specifically 50RH%, 55RH%, 60RH%, 65RH%, 70RH%, 75RH%, 80RH%, 85RH%, 90RH% or any value within the range.

[0049] The pre-evaporation time is 1s to 10min, and can be specifically 1s, 5s, 10s, 20s, 30s, 40s, 50s, 1min, 2min, 3min, 4min, 5min, 6min, 7min, 8min, 9min, 10min or any value within the range.

[0050] The standing time is 1 to 10 minutes, and specifically can be 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes or any value within the range.

[0051] The temperature of the water bath is 15-70°C, specifically 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, 65°C, 70°C or any value within the range.

[0052] The invention also discloses a composite diaphragm for producing hydrogen by electrolyzing water, which is prepared according to the method.

[0053] After testing, its surface resistance is <0.5Ω / cm 2 , static contact angle is less than 70°, wet tensile strength is greater than 20N / mm 2 .

[0054] According to the stability test, the composite diaphragm prepared by the present invention has excellent quality stability, surface resistance stability and tensile strength stability in alkaline solution. After being immersed in a 30% KOH aqueous solution at 90°C for 30 days, the quality change rate is no more than 1.0%, the surface resistance change rate is less than 1.0%, and the wet tensile strength change rate is no more than 1.2%.

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] The invention discloses a method for preparing a composite diaphragm for producing hydrogen by electrolysis of water, wherein polyphenylene sulfide is used as a substrate of the composite diaphragm, zirconium oxide is used as a hydrophilic material, zirconium oxide is modified, and a polymer resin such as polysulfone is used as a binder to mix with the modified zirconium oxide to prepare a slurry, and the slurry is coated on both sides of the polyphenylene sulfide net, and a composite diaphragm is prepared after phase conversion, and the method can significantly improve the bonding force between zirconium oxide and polyphenylene sulfide, on the one hand, solve the problem of shedding after long-term operation caused by directly mixing zirconium oxide and polyphenylene sulfide in the prior art, and on the other hand, a composite diaphragm with excellent hydrophilicity, excellent mechanical properties, low surface resistance, and excellent alkali solution stability can be prepared. The preparation process is simple, controllable, and easy to implement. DETAILED DESCRIPTION

[0057] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.

[0058] Example 1

[0059] 1) Zirconia modification

[0060] Commercially available zirconium oxide powder (Oriental Zirconium, specific surface area = 50 m 2 / g, D50=3μm) was placed in a 20wt% sodium hydroxide aqueous solution, heated at 90°C for 12h, then filtered, washed with water, and dried in an oven at 100°C for 2h.

[0061] After testing, the surface hydroxyl density of modified zirconium oxide was 6nOH / nm 2 .

[0062] 2) Slurry preparation

[0063] Weigh 48 g of polysulfone resin PSU (weight average molecular weight 40,000, distribution index 3-4), slowly add it into 240 mL of NMP, stir at 300 rpm for 12 h, then slowly add 192 g of the above-mentioned modified zirconia, continue to stir at 300 rpm in vacuum for 12 h, control the absolute pressure to 1 kPa, and obtain a white slurry.

[0064] 3) Diaphragm preparation

[0065] The white slurry was coated on both sides of a 300 mm wide PPS mesh (0.28 mm thick, 50 mesh) using a slot die coating technique at a coating speed of 0.5 m / min. After coating, it was pre-evaporated in air (temperature 25°C, humidity 90 RH%) for 15 seconds, and then placed in a 40°C water bath for 5 minutes for phase inversion. After removal, it was washed and rolled up.

[0066] Example 2

[0067] The preparation process is basically the same as that in Example 1, except that in step 1):

[0068] Commercially available zirconium oxide powder was placed in a 10 wt % sodium hydroxide aqueous solution and heated at 80° C. for 3 h.

[0069] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this embodiment is 1nOH / nm 2 .

[0070] Example 3

[0071] The preparation process is basically the same as that in Example 1, except that in step 1):

[0072] Using specific surface area = 10m 2 / g, D50=3μm commercially available zirconium oxide powder (Oriental Zirconium Industry), and the concentration of the sodium hydroxide aqueous solution was replaced with 30wt%.

[0073] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this embodiment is 6nOH / nm 2 .

[0074] Example 4

[0075] The preparation process is basically the same as that in Example 1, except that in step 1):

[0076] Specific surface area = 50m 2 / g, commercially available zirconium oxide powder (Oriental Zirconium Industry), D50=0.5μm.

[0077] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this embodiment is 6nOH / nm 2 .

[0078] Example 5

[0079] The preparation process is basically the same as that in Example 1, except that in step 2), when preparing the slurry:

[0080] 48 g of polysulfone resin PSU was weighed and slowly added into 240 mL of NMP, and stirred at 300 rpm for 12 h. Then 72 g of modified zirconium oxide was slowly added, and stirring was continued at 300 rpm for 12 h to obtain a white slurry.

[0081] Example 6

[0082] The preparation process is basically the same as that in Example 1, except that in step 2), when preparing the slurry:

[0083] Weigh 48 g of polysulfone resin PSU (weight average molecular weight 40,000, distribution index 3-4), slowly add it into 240 mL of NMP, stir at 300 rpm for 12 h, then slowly add 432 g of the above-mentioned modified zirconia, continue to stir at 300 rpm in vacuum for 12 h, control the absolute pressure to 1 kPa, and obtain a white slurry.

[0084] Example 7

[0085] The preparation process is basically the same as that in Example 1, except that in step 2), when preparing the slurry:

[0086] Weigh 48 g of polysulfone resin PSU (weight average molecular weight 40,000, distribution index 3-4), slowly add it into 240 mL of NMP, stir at 300 rpm for 12 h, then slowly add 72 g of the above-mentioned modified zirconia, continue to stir at 300 rpm in vacuum for 12 h, control the absolute pressure to 1 kPa, and obtain a white slurry.

[0087] Example 8

[0088] The preparation process is basically the same as that in Example 1, except that in step 2), when preparing the slurry:

[0089] The polysulfone resin was replaced by an equal mass of polyethersulfone resin PES (BASF Ultrason E2010), and NMP was replaced by an equal volume of N,N-dimethylformamide (DMF).

[0090] After testing, the performance indicators of the composite membrane finally prepared were close to those of Example 1.

[0091] Comparative Example 1

[0092] The preparation process is basically the same as that in Example 1, except that in step 1):

[0093] Commercially available zirconium oxide powder was placed in a 5 wt % sodium hydroxide aqueous solution and heated at 60° C. for 1 h.

[0094] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this comparative example is 0.5nOH / nm 2 .

[0095] Comparative Example 2

[0096] The preparation process is basically the same as that in Example 1, except that in step 1):

[0097] Commercially available zirconium oxide powder was placed in a 30 wt % sodium hydroxide aqueous solution and heated at 95° C. for 24 h.

[0098] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this comparative example is 10nOH / nm 2 .

[0099] Comparative Example 3

[0100] The preparation process is basically the same as that in Example 1, except that in step 1):

[0101] Using specific surface area = 100m 2 / g, D50=3μm commercially available zirconium oxide powder (Oriental Zirconium Industry), and the concentration of the sodium hydroxide aqueous solution was replaced with 15wt%.

[0102] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this comparative example is 6nOH / nm 2 .

[0103] Comparative Example 4

[0104] The preparation process is basically the same as that in Example 1, except that in step 1):

[0105] Using specific surface area = 5m 2 / g, D50=3μm commercially available zirconium oxide powder (Oriental Zirconium Industry), and the concentration of the sodium hydroxide aqueous solution was replaced with 35wt%.

[0106] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this comparative example is 6nOH / nm 2 .

[0107] Comparative Example 5

[0108] The preparation process is basically the same as that in Example 1, except that in step 1):

[0109] Using specific surface area = 50m 2 / g, commercially available zirconium oxide powder (Oriental Zirconium Industry), D50=0.1μm.

[0110] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this comparative example is 6nOH / nm 2 .

[0111] Comparative Example 6

[0112] The preparation process is basically the same as that in Example 1, except that in step 1):

[0113] Using specific surface area = 50m 2 / g, commercially available zirconium oxide powder (Oriental Zirconium Industry), D50=10μm.

[0114] After testing, the surface hydroxyl density of the modified zirconium oxide prepared in step 1) of this comparative example is 6nOH / nm 2 .

[0115] Performance Testing

[0116] The surface hydroxyl density of the modified zirconium oxide prepared in each embodiment or comparative example was tested, and the surface resistance, contact angle, mechanical properties and stability of the composite diaphragm prepared in each embodiment or comparative example were tested.

[0117] 1. Surface hydroxyl density test:

[0118] The hydroxyl density on the surface of the hydrophilic particles is calculated using the following formula, where α is the correction factor, which is 0.625 for zirconium oxide, Na is the Avogadro constant, and MW H2O is the molecular mass of water, S is the specific surface area, wt T1 is the mass of modified zirconia at 450°C, wt T2 is the mass of modified zirconia at 800°C, wt T1 and wt T2 Measured by TGA.

[0119]

[0120] 2. Surface resistance test:

[0121] Refer to SJ / T 10171-2016 standard. Before testing, the composite membranes prepared in each embodiment or comparative example were immersed in a 30wt% KOH aqueous solution for 24h. The test solution was a 30wt% KOH aqueous solution at 23℃±2℃. The resistance was tested with an AC low impedance meter, and the surface resistance R s The calculation formula is as follows: R1 is the solution resistance when the membrane is added, and R0 is the blank solution resistance.

[0122] R s =(R1-R0)×A

[0123] 3. Contact angle test:

[0124] The static contact angle of the composite diaphragm is tested according to GB / T 30693-2014 standard.

[0125] 4. Wet tensile strength test:

[0126] The wet tensile strength is tested according to SJ / T 10171-2016 standard.

[0127] 5. Composite diaphragm stability test:

[0128] The composite diaphragms prepared in the embodiments or comparative examples of the same size were placed in a 30 wt % KOH aqueous solution at 90° C. and stirred at 300 rpm for 30 days. After being taken out, they were washed with water and dried, and the changes in total mass, tensile strength and surface resistance were observed.

[0129] All test data are listed in Table 1 below.

[0130] Table 1

[0131]

[0132] By comparing the data in Examples 1 to 4 and Comparative Examples 1 to 6, it can be seen that by controlling the specific surface area, average pore size and surface hydroxyl density of zirconium oxide within a suitable range, the prepared composite diaphragm has excellent hydrophilicity, mechanical properties, alkaline solution stability and low surface resistance.

[0133] By comparing the data of Example 5 with that of Example 7, it can be seen that when the slurry is prepared under vacuum conditions, the zirconium oxide particles of the composite diaphragm finally prepared are better bonded with the polymer resin, have higher tensile strength, and better stability.

[0134] By comparing the data of Examples 1, 6 and 7, it can be seen that when the mass ratio of the polymer resin polysulfone to zirconium oxide is controlled at 1:(1.5-9.0), a composite diaphragm with low surface resistance and high stability can be prepared.

[0135] The applicant declares that the present invention illustrates the detailed method of the present invention through the above embodiments, but the present invention is not limited to the above detailed method.

Claims

1. A method for preparing a composite diaphragm for producing hydrogen by electrolysis of water, characterized in that: The steps include: 1) mixing zirconium oxide powder with an alkaline solution, and heating and modifying the mixture to obtain modified zirconium oxide; The specific surface area of ​​the zirconium oxide powder is 10 to 50 m 2 / g, average particle size D50 is 0.5~3.0μm; The surface hydroxyl density of the modified zirconium oxide obtained after heating modification is (1-6) nOH / nm 2 ; 2) mixing the polymer resin, modified zirconium oxide and an organic solvent, and stirring them evenly to obtain a slurry; 3) coating the slurry on both sides of the polyphenylene sulfide network, and obtaining the composite diaphragm for producing hydrogen by electrolysis of water after phase conversion.

2. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to claim 1, characterized in that: In step 1), the alkaline solution is selected from one or more of a sodium hydroxide aqueous solution, a potassium hydroxide aqueous solution, and a sodium bicarbonate aqueous solution.

3. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to claim 1, characterized in that: In step 1), the heating modification temperature is 60 to 100° C. and the time is 1 to 24 hours.

4. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to claim 1, characterized in that: In step 2): The polymer resin is selected from one or more of polysulfone, polyethersulfone and polyphenylsulfone; The organic solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N-ethyl-pyrrolidone, acetonitrile and dimethyl sulfoxide.

5. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to claim 1, characterized in that: In step 2): The mass ratio of polymer resin to modified zirconium oxide is 1:(1.5-9.0); The mass volume ratio of the polymer resin to the organic solvent is 1: (1-30) g / mL.

6. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to claim 1, characterized in that: In step 3), the phase conversion is specifically: The coated polyphenylene sulfide mesh is placed in air with a humidity of (50-90) RH% for pre-evaporation for 1 second to 10 minutes, and then placed in a water bath for 1 to 10 minutes; The temperature of the water bath is 15-70°C.

7. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to any one of claims 1 to 6, characterized in that: In step 2), all raw materials are stirred evenly under vacuum conditions to obtain a slurry.

8. The method for preparing a composite diaphragm for producing hydrogen by electrolysis of water according to claim 1, characterized in that: In step 2), under the vacuum condition, the absolute pressure is controlled to be ≤10 kPa.

9. A composite diaphragm for producing hydrogen by electrolysis of water prepared according to the method according to any one of claims 1 to 8.

10. A composite diaphragm for producing hydrogen by electrolysis of water according to claim 9, characterized in that: Surface resistance <0.5Ω / cm 2 , static contact angle is less than 70°, wet tensile strength is greater than 23N / mm 2 ; and after being immersed in a 30wt% KOH aqueous solution at 90°C for 30 days, the mass change rate is no more than 1.0%, the surface resistance change rate is less than 1.0%, and the wet tensile strength change rate is no more than 1.2%.

Citation Information

Cited By

  • Modified diaphragm for electrolyzed water as well as preparation method and application of modified diaphragm

    CN119877031A

  • Alkaline electrolytic water hydrogen production diaphragm based on zirconium oxide modification and preparation method thereof

    CN120384308A

  • Diaphragm cloth for electrolytic hydrogen production

    CN120400926A

  • Alkaline electrolyzed water composite diaphragm based on hydroxyl alumina and preparation method of alkaline electrolyzed water composite diaphragm