Terminal and electroplating process
Through the partitioned electroplating process, the use and cost of electroplating materials is reduced for the terminals of new energy electric vehicles, and the problems of large and high cost of electroplating materials are solved, achieving both high electrical performance and environmental resistance.
Patent Information
- Application Number
- CN202410964726.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, electroplating materials are used in large quantities and cost, making it difficult to meet the high electrical performance and environmental resistance requirements of terminals of new energy electric vehicles.
The partitioned electroplating process is adopted, and the terminal surface is divided into the first surface and the second surface. The first surface is electroplating with a thicker base coating and functional coating. The second surface has no plating or the coating is thinner. The second surface is covered by a shielding member for electroplating. Reduce the amount of electroplating material.
Without affecting product performance, the amount of electroplating materials and manufacturing costs are reduced, the material consumption performance is improved, and the electrical performance and environmental resistance requirements of the terminals are met.
Smart Images

Figure CN118932443A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electroplating terminals, and more specifically, to a terminal and an electroplating process. Background Art
[0002] In order to meet the designed charging power and ensure the safety of the charging process, new energy electric vehicles have very high requirements for the electrical performance and environmental resistance of the terminals. They need to meet various test requirements such as contact resistance, temperature rise, durable plugging and unplugging, and salt spray testing.
[0003] In order to achieve the above product performance and quality requirements, traditional terminals generally use a copper terminal that is electroplated with nickel as a whole and then electroplated with silver as a whole. However, the tail of some terminals is designed with a sealing structure that cooperates with other seals such as a waterproof ring. After actual assembly, the waterproof ring will tightly cover the above sealing structure at the tail of the terminal, so that the sealing structure does not need electroplating to have good environmental tolerance. Therefore, based on the above actual situation, it is meaningful to develop and design a new terminal plating structure and electroplating process to reduce the amount of electroplating materials. Summary of the invention
[0004] The invention provides a terminal and an electroplating process to solve the problems of large amount of electroplating materials and high cost in the prior art.
[0005] A terminal provided by the present invention is used to connect with a mating terminal and transmit electrical energy, including a terminal body, the surface of the terminal body including a first surface and a second surface, the second surface is located on the partial outside of the terminal body and is used to seal with a corresponding sealing structure, and a base coating and a functional coating are provided on at least part of the surface of the terminal body; the functional coating is at least located on the first surface and is on the upper layer of the base coating, and the thickness of the functional coating at the first surface is greater than the thickness at other surfaces.
[0006] Optionally, the base coating and the functional coating both cover the first surface, and the second surface has no coating and is sealed with the sealing structure.
[0007] Optionally, the base coating and the functional coating both cover the first surface and the second surface, and the thickness of the functional coating at the first surface is greater than the thickness at the second surface.
[0008] Optionally, the base coating is a nickel / copper coating, and the functional coating is a noble metal / noble metal alloy coating.
[0009] Optionally, the base coating and the functional coating both cover the first surface and the second surface, the noble metal / noble metal alloy coating is a silver-antimony alloy coating, and the thickness of the silver-antimony alloy coating at the first surface is not less than 5 μm and the thickness at the second surface is not more than 3 μm.
[0010] Optionally, the base coating and the functional coating both cover the first surface, the second surface is uncoated and is sealed with the sealing structure, the precious metal / precious metal alloy coating is a silver-antimony alloy coating, and the thickness of the silver-antimony alloy coating is not less than 5 μm.
[0011] Optionally, the base coating is a nickel coating, and the thickness of the nickel coating is 3-5 μm.
[0012] The present invention provides an electroplating process for manufacturing the terminal as described above, comprising the following steps:
[0013] a. Partition: define the first surface and the second surface of the terminal;
[0014] b. Pre-plating treatment: remove impurities on the terminal surface;
[0015] c. Electroplating a base plating layer: immersing at least a portion of the first surface of the terminal in a base plating solution for electroplating to obtain a base plating layer covering at least the first surface;
[0016] d. Shielding: Covering the second surface of the terminal by a shielding member;
[0017] e. Electroplating a functional coating: immersing a portion of the first surface of the terminal in a functional electroplating solution for electroplating to obtain a functional coating;
[0018] f. Post-plating protection: immerse the terminals in protective agent;
[0019] g. Dry the terminals after removing the shielding parts.
[0020] Optionally, the step c includes: immersing the entire terminal in a base plating solution for electroplating to obtain a base plating layer covering the first surface and the second surface; the step between step c and step d also includes the following steps: c1, pre-plating: immersing the entire terminal in a functional plating solution for electroplating to obtain a functional plating layer of basic form covering the first surface and the second surface; the step e includes: immersing part of the first surface of the terminal in a functional plating solution for electroplating to increase the thickness of the functional plating layer of basic form on the first surface part to obtain the functional plating layer of final form.
[0021] Optionally, the electroplating time in step c1 is 5-20 min, and the electroplating time in step e is 20-85 min.
[0022] Optionally, step c includes: using a shielding member to cover the outer side of the second surface of the terminal, immersing the entire terminal in a base plating solution for electroplating, and obtaining a base plating layer covering the first surface; step d includes: maintaining a state in which the shielding member covers the second surface of the terminal.
[0023] Optionally, the shielding member is a silicone sleeve, and the silicone sleeve is installed on the terminal to shield the second surface of the terminal.
[0024] Optionally, the base electroplating solution is a nickel electroplating solution, which contains, based on the total volume of the electroplating solution, 300-450 g / L of nickel sulfamate, 2-15 g / L of nickel chloride, 30-45 g / L of boric acid, a pH value of 3.5-4.5, an electroplating temperature of 40-60° C., and an electroplating current density of 1-5 A / dm 2 , the electroplating time is 20-35min; the functional electroplating solution adopts silver antimony electroplating solution, and based on the total volume of the electroplating solution, the silver antimony electroplating solution contains silver nitrate: 35-45g / L, potassium cyanide: 80-90g / L, potassium sodium tartrate: 40-50g / L, potassium antimony tartrate 1.5-3g / L, pH value is 3.5-4.5, electroplating temperature is 18-22℃, and current density is 1-2A / dm 2 , the electroplating time is 30-90min.
[0025] Optionally, step b includes:
[0026] b1. Ultrasonic degreasing: ultrasonic degreasing of the terminals;
[0027] b2. Electrolytic degreasing: Electrolytic degreasing of the terminals;
[0028] b3. Pickling: Use acid solution to clean the terminals.
[0029] The present invention has the following beneficial effects:
[0030] The terminal surface is divided into a first surface and a second surface. A thicker plating layer that can achieve a predetermined function is electroplated on the first surface, and then a thinner plating layer can be electroplated on the second surface that is sealed with a sealing structure, or the plating layer can be left unplated after shielding, thereby reducing the amount of plating materials and manufacturing costs without affecting product performance.
[0031] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0033] Figure 1 is a schematic diagram of the structure of the terminal;
[0034] Figure 2 This is a schematic diagram of the terminal shielding state;
[0035] Figure 3 A schematic diagram of a coating structure in which a base coating and a functional coating only cover a first surface;
[0036] Figure 4 It is a schematic diagram of the coating structure in which the base coating and the functional coating both cover the first surface and the second surface.
[0037] The following are marked in the figure:
[0038] 1. Terminal; 11. Terminal body; 2. First surface; 3. Second surface; 4. Silicone sleeve; 5. Base coating; 6. Functional coating; 61. Base layer; 62. Thickening layer. DETAILED DESCRIPTION
[0039] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0040] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0041] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0042] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0043] Example 1.
[0044] like Figure 1 , Figure 3 As shown, a terminal 1 is used to connect with a mating terminal and transmit electrical energy, including a terminal body 11. The surface of the terminal body 11 includes a first surface 2 and a second surface 3. The second surface 3 is located on the outer side of a portion of the terminal body 11 and is used to seal with a corresponding sealing structure, such as a waterproof ring or a sealing ring preset in a sheath. The terminal is inserted into the sealing structure and the second surface 3 is fitted with the sealing structure to achieve a sealed fit. A base coating 5 and a functional coating 6 are provided on at least part of the surface of the terminal body 11; the functional coating 6 is located at least on the first surface 2 and is in the upper layer of the base coating 5, and the thickness of the functional coating 6 at the first surface 2 is greater than the thickness at other surfaces.
[0045] In this embodiment, the base coating 5 and the functional coating 6 both cover the first surface 2, and the second surface 3 has no coating and is in sealing cooperation with the sealing structure.
[0046] Furthermore, the base coating 5 is a nickel / copper coating, and the functional coating 6 is a precious metal / precious metal alloy coating. Preferably, according to actual use requirements, in this embodiment, the base coating 5 is a nickel coating, and the functional coating 6 is a silver-antimony alloy coating.
[0047] In order to ensure the electrical performance and environmental resistance, meet the needs of electroplating, and improve the cost-effectiveness of material consumption, the thickness of the nickel plating layer is more reasonably in the range of 3-5μm, the thickness of the silver-antimony alloy plating layer at the first surface 2 is more reasonable to be not less than 5μm, and the more reasonable range is 5-15μm, and the thickness at the second surface 3 is more reasonable to be no more than 3μm. When the thickness of each plating layer is small, the product performance is poor, which is suitable for occasions with lower requirements and less electroplating material consumption. When the thickness of each plating layer is high, the product performance is better, which is suitable for occasions with higher requirements, and the corresponding electroplating material consumption is more. In practice, flexible selection can be made within the above thickness range according to needs.
[0048] In this embodiment, the thickness of the nickel plating layer is 3 μm, the thickness of the silver-antimony alloy plating layer on the first surface 2 is 5 μm, and the thickness on the second surface 3 is 0 μm, that is, there is no silver-antimony alloy plating layer.
[0049] An electroplating process for manufacturing the above-mentioned terminal comprises the following steps:
[0050] a. Partition: define the first surface and the second surface of the terminal;
[0051] b. Pre-plating treatment: remove impurities on the terminal surface;
[0052] c. electroplating a base plating layer: immersing at least a portion of the first surface of the terminal in a base plating solution to obtain a base plating layer covering at least the first surface;
[0053] d. Shielding: Covering the second surface of the terminal by a shielding member;
[0054] e. Electroplating a functional coating: immersing a portion of the first surface of the terminal in a functional electroplating solution for electroplating to obtain a functional coating;
[0055] f. Post-plating protection: immerse the terminals in protective agent;
[0056] g. Dry the terminals after removing the shielding parts.
[0057] In this embodiment, considering that the second surface does not need to be plated, step c actually includes: using a shielding member to cover the outside of the second surface of the terminal, immersing the entire terminal in a base plating solution, and obtaining a base plating layer covering the first surface; step d actually includes: maintaining a state in which the shielding member covers the second surface of the terminal.
[0058] The shielding member can be a tape, a rubber sleeve or other device according to the actual situation and the terminal structure. In this embodiment, the shielding member is a silicone sleeve. In step c, the silicone sleeve 4 with a suitable shape is actually set on the second surface of the terminal to shield the second surface. Figure 2 As shown, in step e, the entire terminal is actually immersed in the functional plating solution.
[0059] In this embodiment, the base plating solution in step c is a nickel plating solution, and the specific ratio is: based on the total volume of the plating solution, the nickel plating solution contains nickel sulfamate: 400g / L (reference selection range: 300-450g / L), nickel chloride: 8g / L (reference selection range: 2-15g / L), boric acid: 40g / L (reference selection range: 30-45g / L), pH value: 4.0 (reference selection range: 3.5-4.5). The plating parameters in the electroplating are: the plating temperature is: 55°C (reference selection range: 40-60°C), the plating current density is: 3A / dm 2 (Reference selection range: 1-5A / dm 2 ), electroplating time: 20min (reference selection range: 20-35min).
[0060] In this embodiment, the functional electroplating solution in step e is a silver antimony electroplating solution, and the specific ratio is: based on the total volume of the electroplating solution, the silver antimony electroplating solution contains silver nitrate: 40g / L (reference selection range: 35-45g / L), potassium cyanide: 85g / L (reference selection range: 80-90g / L), potassium sodium tartrate: 45g / L (reference selection range: 40-50g / L), potassium antimony tartrate: 2.5g / L (reference selection range: 1.5-3g / L), pH value: 4.0 (reference selection range: 3.5-4.5). The electroplating parameters in the electroplating are: the electroplating temperature is: 20°C (reference selection range: 18-22°C), the electroplating current density is: 1.5A / dm 2 (Reference selection range: 1-2A / dm 2 ), electroplating time: 30min (reference selection range: 30-90min).
[0061] In this embodiment, the protective agent in step f is a silver post-plating protective agent suitable for post-plating protection of silver-plated layers. It is a conventional material and technology in the field, so it is not described in detail.
[0062] It is apparent to those skilled in the art that the ratio of the above-mentioned electroplating solution and the electroplating parameters can be flexibly selected and combined within the range shown according to actual conditions, so as to ultimately electroplate a coating thickness that meets the requirements.
[0063] In this embodiment, in order to ensure the cleanliness of the surface of the terminal body to the greatest extent, step b includes:
[0064] b1. Ultrasonic degreasing: ultrasonic degreasing of the terminals, ultrasonic degreasing solution ratio and parameters: sodium hydroxide: 13g / L (reference selection range: 10-15g / L), sodium carbonate: 25g / L (reference selection range: 20-30g / L), trisodium phosphate: 60g / L (reference selection range: 50-70g / L), sodium silicate: 13g / L (reference selection range: 10-15g / L), temperature: 60℃ (reference selection range: 50-70℃), time: 12min (reference selection range: 8-16min);
[0065] b2. Electrolytic degreasing: Electrolytic degreasing of the terminals, electrolytic degreasing solution ratio and parameters: sodium hydroxide: 13g / L (reference selection range: 10-15g / L), sodium carbonate: 25g / L (reference selection range: 20-30g / L), sodium phosphate: 60g / L (reference selection range: 50-70g / L), sodium silicate: 13g / L (reference selection range: 10-15g / L), temperature: 60℃ (reference selection range: 50-70℃), current density: 5A / dm 2 (Reference selection range: 3-8A / dm 2 ), time: 12min (reference selection range: 10-15min);
[0066] b3. Pickling: Use an acid solution to clean the terminals. The ratio and parameters of the acid solution are as follows: sulfuric acid (volume ratio): 15% (reference selection range: 10%-20%), time: 70s (preferred parameters: 60-90s).
[0067] Among them, after the steps b1, b2 and b3 are completed, a water washing process is performed, in which pure water is used for washing, the conductivity of the pure water is required to be less than 10 μS / cm, and the washing time is 60 s.
[0068] In the above-mentioned terminal and electroplating process, the surface of the terminal body is divided into a first surface and a second surface. A thicker plating layer that can achieve a predetermined function is plated on the first surface. Then, the second surface that seals with the sealing structure can be masked and not plated, thereby reducing the amount of electroplating materials and manufacturing costs without affecting product performance.
[0069] As a further improvement, in order to reduce the adverse effects of the nickel-silver replacement reaction on the nickel plating layer caused by the nickel plating layer directly entering the silver-antimony electroplating solution and improve the stability between the nickel plating layer and the silver-antimony alloy plating layer, in this embodiment, a step e0 can also be added between step d and step e. Step e0 includes: immersing the entire terminal in the silver plating solution for electroplating to form a protective silver film covering the nickel plating layer. Therefore, when step e is subsequently performed, the silver film blocks the nickel plating layer and the silver-antimony electroplating solution, avoiding or reducing the adverse effects of the replacement reaction. The silver-antimony alloy plating layer as a functional plating layer is actually plated on the silver film.
[0070] In step e0, the proportion of the silver electroplating solution can be: based on the total volume of the electroplating solution, the silver electroplating solution contains silver cyanide: 3-5g / L, potassium cyanide: 60-70g / L, potassium carbonate: 5-10g / L, and the pH value is 3.5-4.5. The electroplating parameters in the electroplating are: the electroplating temperature is 18-30°C, the current density is 0.3-0.5A / dm 2 , the plating time is 20-60s.
[0071] Example 2.
[0072] The difference between this embodiment and the above-mentioned embodiment 1 lies in the thickness of the nickel plating layer and the silver-antimony alloy plating layer, and the time parameter of the electroplating in the electroplating process, which are as follows.
[0073] In this embodiment, the thickness of the nickel plating layer is 4 μm, and the thickness of the silver-antimony alloy plating layer is 10 μm.
[0074] In this embodiment, the time parameters in the nickel plating layer electroplating are: electroplating time: 26 minutes.
[0075] In this embodiment, the time parameters in the electroplating of the silver-antimony alloy coating are: the electroplating time is: 60 minutes.
[0076] The coating thickness of this embodiment is greater than that of the embodiment 1, and the electrical performance and environmental resistance are improved compared with the terminal of the embodiment 1.
[0077] Example 3.
[0078] The difference between this embodiment and the above-mentioned embodiment 1 lies in the thickness of the nickel plating layer and the silver-antimony alloy plating layer, and the time parameter of the electroplating in the electroplating process, which are as follows.
[0079] In this embodiment, the thickness of the nickel plating layer is 5 μm, and the thickness of the silver-antimony alloy plating layer is 15 μm.
[0080] In this embodiment, the time parameters in the nickel plating layer electroplating are: electroplating time: 33 minutes.
[0081] In this embodiment, the time parameters in the electroplating of the silver-antimony alloy coating are: the electroplating time is: 90 minutes.
[0082] The coating thickness of this embodiment is greater than that of the embodiment 2, and the electrical performance and environmental resistance are improved compared with the terminal of the embodiment 2.
[0083] Example 4.
[0084] A terminal of the present embodiment is used to connect with a mating terminal and transmit electrical energy, including a terminal body. The surface of the terminal body includes a first surface and a second surface. The second surface is located on the outer side of a portion of the terminal body and is used to seal with a corresponding sealing structure, such as a waterproof ring or a sealing ring preset in a sheath. The terminal is inserted into the sealing structure and the second surface is fitted with the sealing structure to achieve a sealed fit. A base coating and a functional coating are provided on at least part of the surface of the terminal body; the functional coating is at least located on the first surface and is on the upper layer of the base coating, and the thickness of the functional coating at the first surface is greater than the thickness at other surfaces.
[0085] In this embodiment, Figure 4 As shown, the base coating 5 and the functional coating 6 both cover the first surface 2 and the second surface 3 , and the thickness of the functional coating 6 at the first surface 2 is greater than the thickness at the second surface 3 .
[0086] Furthermore, the base coating is a nickel / copper coating, and the functional coating is a noble metal / noble metal alloy coating. Preferably, according to actual use requirements, in this embodiment, the base coating is a nickel coating, and the functional coating is a silver-antimony alloy coating.
[0087] In order to ensure the electrical performance and environmental resistance, meet the needs of electroplating, and improve the cost-effectiveness of material consumption, the thickness of the nickel plating layer is more reasonable in the range of 3-5μm, the thickness of the silver-antimony alloy plating layer at the first surface is more reasonable to be no less than 5μm, and the more reasonable range is 5-15μm, and the thickness at the second surface is more reasonable to be no more than 3μm. When the thickness of each plating layer is small, the product performance is poor, which is suitable for occasions with lower requirements and less electroplating material consumption. When the thickness of each plating layer is high, the product performance is better, which is suitable for occasions with higher requirements, and the corresponding electroplating material consumption is more. In practice, flexible selection can be made within the above thickness range according to needs.
[0088] In this embodiment, the thickness of the nickel plating layer is 3 μm, the thickness of the silver-antimony alloy plating layer at the first surface is 5 μm, and the thickness of the silver-antimony alloy plating layer at the second surface is 1 μm.
[0089] In this embodiment, a silver-antimony alloy plating layer is also provided on the second surface, and the electrical performance and environmental resistance performance at the second surface are improved compared with the terminal in Embodiment 1.
[0090] An electroplating process for manufacturing the above-mentioned terminal comprises the following steps:
[0091] a. Partition: define the first surface and the second surface of the terminal;
[0092] b. Pre-plating treatment: remove impurities on the terminal surface;
[0093] c. electroplating a base plating layer: immersing at least a portion of the first surface of the terminal in a base plating solution to obtain a base plating layer covering at least the first surface;
[0094] d. Shielding: Covering the second surface of the terminal by a shielding member;
[0095] e. Electroplating a functional coating: immersing a portion of the first surface of the terminal in a functional electroplating solution for electroplating to obtain a functional coating;
[0096] f. Post-plating protection: immerse the terminals in protective agent;
[0097] g. Dry the terminals after removing the shielding parts.
[0098] In this embodiment, considering that the thickness of the functional coating on the second surface is less than that on the first surface, step c actually includes: immersing all the terminals in the base plating solution for electroplating to obtain a base coating covering the first surface and the second surface.
[0099] In this embodiment, the steps between step c and step d include: c1, pre-plating: immersing the entire terminal in a functional plating solution for electroplating to obtain a functional plating layer covering the first surface and the second surface in a basic form, that is, Figure 4 The base layer 61 is shown.
[0100] In this embodiment, step e includes: immersing a portion of the first surface of the terminal in a functional electroplating solution for electroplating, thereby increasing the thickness of the functional plating layer of the basic form on the first surface portion, such as Figure 4 As shown, a thickening layer 62 is formed on the base layer, and the thickening layer 62 and the base layer 61 together form a functional coating layer 6, and finally the functional coating layer 6 in a final form is obtained.
[0101] The shielding member can be a device such as tape, rubber sleeve, etc. according to the actual situation and terminal structure. In this embodiment, the shielding member is a silicone sleeve. In step d, a silicone sleeve with a matching shape is actually set on the second surface of the terminal to shield the second surface.
[0102] In this embodiment, the base plating solution in step c is a nickel plating solution, and the specific ratio is: based on the total volume of the plating solution, the nickel plating solution contains nickel sulfamate: 400g / L (reference selection range: 300-450g / L), nickel chloride: 8g / L (reference selection range: 2-15g / L), boric acid: 40g / L (reference selection range: 30-45g / L), pH value: 4.0 (reference selection range: 3.5-4.5). The plating parameters in the electroplating are: the plating temperature is: 55°C (reference selection range: 40-60°C), the plating current density is: 3A / dm 2 (Reference selection range: 1-5A / dm 2 ), electroplating time: 20min (reference selection range: 20-35min).
[0103] In this embodiment, the functional electroplating solution in step c1 and step e is a silver antimony electroplating solution, and the specific ratio is: based on the total volume of the electroplating solution, the silver antimony electroplating solution contains silver nitrate: 40g / L (reference selection range: 35-45g / L), potassium cyanide: 85g / L (reference selection range: 80-90g / L), potassium sodium tartrate: 45g / L (reference selection range: 40-50g / L), potassium antimony tartrate: 2.5g / L (reference selection range: 1.5-3g / L), pH value: 4.0 (reference selection range: 3.5-4.5). The electroplating parameters in step c1 are: electroplating temperature: 20°C (reference selection range: 18-22°C), electroplating current density: 1.5A / dm 2 (Reference selection range: 1-2A / dm 2 ), electroplating time: 6min (reference selection range: 5-20min), electroplating parameters in step e are: electroplating temperature: 20℃ (reference selection range: 18-22℃), electroplating current density: 1.5A / dm 2 (Reference selection range: 1-2A / dm 2 ), electroplating time: 24min (reference selection range: 20-85min). Among them, the total electroplating time in the silver antimony electroplating solution is 30min (reference selection range: 30-90min).
[0104] In this embodiment, the protective agent in step f is a silver post-protective agent suitable for silver plating, which is a conventional material and technology in the field, so it is not described in detail.
[0105] It is apparent to those skilled in the art that the ratio of the above-mentioned electroplating solution and the electroplating parameters can be flexibly selected and combined within the range shown according to actual conditions, so as to ultimately electroplate a coating thickness that meets the requirements.
[0106] In this embodiment, in order to ensure the cleanliness of the surface of the terminal body to the greatest extent, step b includes:
[0107] b1. Ultrasonic degreasing: ultrasonic degreasing of the terminals, ultrasonic degreasing solution ratio and parameters: sodium hydroxide: 13g / L (reference selection range: 10-15g / L), sodium carbonate: 25g / L (reference selection range: 20-30g / L), trisodium phosphate: 60g / L (reference selection range: 50-70g / L), sodium silicate: 13g / L (reference selection range: 10-15g / L), temperature: 60℃ (reference selection range: 50-70℃), time: 12min (reference selection range: 8-16min);
[0108] b2. Electrolytic degreasing: Electrolytic degreasing of the terminals, electrolytic degreasing solution ratio and parameters: sodium hydroxide: 13g / L (reference selection range: 10-15g / L), sodium carbonate: 25g / L (reference selection range: 20-30g / L), sodium phosphate: 60g / L (reference selection range: 50-70g / L), sodium silicate: 13g / L (reference selection range: 10-15g / L), temperature: 60℃ (reference selection range: 50-70℃), current density: 5A / dm 2 (Reference selection range: 3-8A / dm 2 ), time: 12min (reference selection range: 10-15min);
[0109] b3. Pickling: Use an acid solution to clean the terminals. The ratio and parameters of the acid solution are as follows: sulfuric acid (volume ratio): 15% (reference selection range: 10%-20%), time: 70s (preferred parameters: 60-90s).
[0110] Among them, after the steps b1, b2 and b3 are completed, a water washing process is performed, in which pure water is used for washing, the conductivity of the pure water is required to be less than 10 μS / cm, and the washing time is 60 s.
[0111] In the above-mentioned terminals and electroplating process, the surface of the terminal body is divided into a first surface and a second surface. A base plating layer and a thicker plating layer that can achieve a predetermined function are electroplated on the first surface, and a base plating layer and a thinner functional plating layer are electroplated on the second surface that seals with the sealing structure, thereby reducing the amount of electroplating material at the second surface. Without affecting product performance, the amount of electroplating material used and the manufacturing cost of the terminal are reduced.
[0112] As a further improvement, in order to reduce the adverse effects of the nickel-silver replacement reaction on the nickel plating layer caused by the nickel plating layer directly entering the silver-antimony electroplating solution and improve the stability between the nickel plating layer and the silver-antimony alloy plating layer, in this embodiment, a step c0 can also be added between step c and step c1, and step c0 includes: immersing part of the first surface of the terminal in the silver electroplating solution for electroplating to form a protective silver film covering the nickel plating layer. Therefore, when step c1 is subsequently performed, the silver film blocks the nickel plating layer and the silver-antimony electroplating solution, avoiding or reducing the adverse effects of the replacement reaction, and the silver-antimony alloy plating layer as a functional plating layer is actually plated on the silver film.
[0113] In step e0, the proportion of the silver electroplating solution can be: based on the total volume of the electroplating solution, the silver electroplating solution contains silver cyanide: 3-5g / L, potassium cyanide: 60-70g / L, potassium carbonate: 5-10g / L, and the pH value is 3.5-4.5. The electroplating parameters in the electroplating are: the electroplating temperature is 18-30°C, the current density is 0.3-0.5A / dm 2 , the plating time is 20-60s.
[0114] Example 5.
[0115] The difference between this embodiment and the above-mentioned embodiment 4 lies in the thickness of the nickel plating layer and the silver-antimony alloy plating layer, and the time parameter of the electroplating in the electroplating process, which are as follows.
[0116] In this embodiment, the thickness of the nickel plating layer is 4 μm, the thickness of the silver-antimony alloy plating layer at the first surface is 10 μm, and the thickness at the second surface is 2 μm.
[0117] In this embodiment, the time parameters in the nickel plating layer electroplating are: electroplating time: 26 minutes.
[0118] In this embodiment, the time parameters in the electroplating of the silver-antimony alloy coating are: the electroplating time in step c1 is 12 minutes; the electroplating parameters in step e is 48 minutes. The total electroplating time in the silver-antimony electroplating solution is 60 minutes.
[0119] The coating thickness of this embodiment is greater than that of the embodiment 4, and the electrical performance and environmental resistance are improved compared with the terminal of the embodiment 4.
[0120] Example 6.
[0121] The difference between this embodiment and the above-mentioned embodiment 4 lies in the thickness of the nickel plating layer and the silver-antimony alloy plating layer, and the time parameter of the electroplating in the electroplating process, which are as follows.
[0122] In this embodiment, the thickness of the nickel plating layer is 5 μm, the thickness of the silver-antimony alloy plating layer at the first surface is 15 μm, and the thickness at the second surface is 3 μm.
[0123] In this embodiment, the time parameters in the nickel plating layer electroplating are: electroplating time: 33 minutes.
[0124] In this embodiment, the time parameters in the electroplating of the silver-antimony alloy coating are: the electroplating time in step c1 is 18 minutes; the electroplating parameters in step e is 72 minutes. The total electroplating time in the silver-antimony electroplating solution is 90 minutes.
[0125] The coating thickness of this embodiment is greater than that of the embodiment 5, and the electrical performance and environmental resistance are improved compared with the terminal of the embodiment 5.
[0126] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A terminal used to connect with a mating terminal and transfer electrical energy. It is characterized in that It includes a terminal body, the surface of the terminal body includes a first surface and a second surface, the second surface is located on the outside of part of the terminal body and is used to seal with the corresponding sealing structure, and a base coating and a functional coating are provided on at least part of the surface of the terminal body; the functional coating is located at least on the first surface and is on the upper layer of the base coating, and the thickness of the functional coating at the first surface is greater than the thickness at other surfaces.
2. A terminal as claimed in claim 1, It is characterized in that The base coating and the functional coating both cover the first surface, and the second surface has no coating and is sealed with the sealing structure.
3. A terminal as claimed in claim 1, It is characterized in that The base coating and the functional coating both cover the first surface and the second surface, and the thickness of the functional coating at the first surface is greater than the thickness at the second surface.
4. A terminal as claimed in claim 1, It is characterized in that The base coating is a nickel / copper coating, and the functional coating is a noble metal / noble metal alloy coating.
5. A terminal as claimed in claim 4, It is characterized in that The base coating and the functional coating both cover the first surface and the second surface. The noble metal / noble metal alloy coating is a silver-antimony alloy coating. The thickness of the silver-antimony alloy coating at the first surface is not less than 5 μm and the thickness at the second surface is not more than 3 μm.
6. A terminal as claimed in claim 4, It is characterized in that The base coating and the functional coating both cover the first surface, the second surface has no coating and is sealed with the sealing structure, the precious metal / precious metal alloy coating is a silver-antimony alloy coating, and the thickness of the silver-antimony alloy coating is not less than 5 μm.
7. A terminal as claimed in claim 4, It is characterized in that The base plating layer is a nickel plating layer, and the thickness of the nickel plating layer is 3-5 μm.
8. An electroplating process for manufacturing the terminal as claimed in claims 1 to 7, It is characterized in that The steps include: a. Partition: define the first surface and the second surface of the terminal; b. Pre-plating treatment: remove impurities on the terminal surface; c. Electroplating a base plating layer: immersing at least a portion of the first surface of the terminal in a base plating solution for electroplating to obtain a base plating layer covering at least the first surface; d. Shielding: Covering the second surface of the terminal by a shielding member; e. Electroplating a functional coating: immersing a portion of the first surface of the terminal in a functional electroplating solution for electroplating to obtain a functional coating; f. Post-plating protection: immerse the terminals in protective agent; g. Dry the terminals after removing the shielding parts.
9. An electroplating process as claimed in claim 8, It is characterized in that The step c comprises: immersing the entire terminal in a base plating solution for electroplating to obtain a base plating layer covering the first surface and the second surface; the step between the step c and the step d also comprises the steps of: c1, pre-plating: immersing the entire terminal in a functional plating solution for electroplating to obtain a functional plating layer of a basic form covering the first surface and the second surface; the step e comprises: immersing part of the first surface of the terminal in a functional plating solution for electroplating to increase the thickness of the functional plating layer of the basic form on the first surface part to obtain the functional plating layer of the final form.
10. An electroplating process as claimed in claim 9, It is characterized in that The electroplating time in step c1 is 5-20 minutes, and the electroplating time in step e is 20-85 minutes.
11. An electroplating process as claimed in claim 8, It is characterized in that The step c comprises: using a shielding member to cover the outer side of the second surface of the terminal, immersing the entire terminal in a base plating solution for electroplating, and obtaining a base plating layer covering the first surface; the step d comprises: maintaining the state in which the shielding member covers the second surface of the terminal.
12. An electroplating process according to any one of claims 8 to 11, It is characterized in that The shielding member is a silicone sleeve, and the silicone sleeve is installed on the terminal to shield the second surface of the terminal.
13. An electroplating process according to any one of claims 8 to 11, It is characterized in that The base electroplating solution is a nickel electroplating solution. Based on the total volume of the electroplating solution, the nickel electroplating solution contains 300-450 g / L of nickel sulfamate, 2-15 g / L of nickel chloride, 30-45 g / L of boric acid, a pH value of 3.5-4.5, an electroplating temperature of 40-60° C., and an electroplating current density of 1-5 A / dm 2 , the electroplating time is 20-35min; the functional electroplating solution adopts silver antimony electroplating solution, which contains silver nitrate: 35-45g / L, potassium cyanide: 80-90g / L, potassium sodium tartrate: 40-50g / L, potassium antimony tartrate 1.5-3g / L, pH value is 3.5-4.5, electroplating temperature is 18-22°C, current density is 1-2A / dm2, and electroplating time is 30-90min.
14. An electroplating process as claimed in claim 8, It is characterized in that The step b comprises: b1. Ultrasonic degreasing: ultrasonic degreasing of the terminals; b2. Electrolytic degreasing: Electrolytic degreasing of the terminals; b3. Pickling: Use acid solution to clean the terminals.
Citation Information
Cited By
Terminal and electroplating process
WO2026016779A1
Selectively electroplated terminal, selective electroplating process, and electroplating device
WO2026016781A1