Method for electro-deposition of UO2 by liquid electrode
By using liquid bismuth electrodes and high-temperature molten salt systems during oxide electrodeposition, the problem of UO2 shedding was solved, efficient recycling and low-cost production were achieved, and the yield reached 67.7%.
Patent Information
- Application Number
- CN202410989925.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
During the existing oxide electrodeposition process, UO2 on the solid electrode is prone to fall off and fall into the molten salt, resulting in difficulty in recycling and low production efficiency.
The liquid bismuth electrode is used as the cathode, and electrodeposition is carried out through a high-temperature molten salt system. The dendrite-free UO2 is prepared by using a two-step single electron transfer reaction to prevent UO2 from falling off and achieve efficient recovery of UO2.
The dendrite-free generation and efficient recycling of UO2 are achieved, with a yield of 67.7%, while ensuring multiple recycling and easy operation of molten salt, reducing costs and pollution.
Smart Images

Figure CN118932450A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nuclear energy development, and in particular relates to a method for recovering nuclear fuel, namely, electrodepositing UO2. Background Art
[0003] The mainstream nuclear fuel at present is oxide fuel. After being irradiated by the reactor, it is called spent fuel. In order to post-process the spent fuel, the Russian Institute of Atomic Reactors has developed an oxide electrodeposition process. The spent fuel is placed in a molten chloride molten salt system, and chlorine is introduced to convert uranium into uranyl ions UO2. 2+ It exists in the form of UO2 and is finally deposited at the cathode in the form of UO2 through electrolysis. It has reached a semi-industrial state, but the UO2 on the solid electrode is easy to fall off and fall into the molten salt during the electrodeposition process. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems in the existing UO2 electrodeposition process, and use a liquid electrode as a cathode to prevent the UO2 obtained by electrodeposition from falling off into the molten salt.
[0005] Electrochemical principles involved:
[0006] The raw material uranyl fluoride is dissolved in the molten salt to form uranyl ions. When electricity is applied, the process of uranyl ions being electro-reduced to UO2 in the molten salt is a two-step single electron transfer process. Uranium dioxide is prepared through the following cathode reaction:
[0007] UO2 2+ +e - =UO2 +
[0008] UO2 + +e - =UO2.
[0009] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0010] A method for electrodepositing UO2 using a liquid electrode comprises the following steps:
[0011] S1: Preparation of liquid bismuth electrode: a small crucible containing an appropriate amount of Bi particles is placed in a well-type furnace. After Bi is melted, W wire is inserted as a conductor and the W wire is sheathed in a corundum sleeve for protection;
[0012] S2: Molten salt melting and purification: Under an inert atmosphere, a large crucible containing LiCl-KCl eutectic salt is placed in a pit furnace. After the eutectic salt is melted, a three-electrode system is used to pre-electrolyze the molten salt to remove impurities;
[0013] S3: Electrodeposition of uranium dioxide: Under inert atmosphere, add UO2F2 to the pre-electrolyzed molten salt, connect the electrodes to a power source and use a three-electrode system for electrodeposition.
[0014] Furthermore, the purity of the LiCl and KCl is 99.9%.
[0015] Furthermore, the mass ratio of LiCl to KCl is 4.6-4.8:5-5.4.
[0016] Furthermore, the large crucible is a corundum crucible.
[0017] Furthermore, the dimensions of the large crucible are 80 mm in height, 42 mm in bottom diameter, and 67 mm in top diameter.
[0018] Furthermore, the heating of the molten salt to a temperature above the melting point of the molten salt is specifically heating to 500±20°C.
[0019] Furthermore, the three-electrode system is that the anode is a graphite carbon rod, the cathode is a W wire, and the reference electrode is an Ag / AgCl electrode.
[0020] The preparation method of the liquid electrode in step S1 is as follows:
[0021] S11: Preparation of liquid bismuth electrode: Weigh a certain mass of solid Bi particles and put them into a prepared small crucible, then place it in a pit furnace and heat the temperature to above the melting point of Bi;
[0022] S21: When the solid Bi is completely melted into liquid, the treated W wire is inserted into the liquid Bi as an electrical conductor, and then the crucible is taken out of the pit furnace;
[0023] S31: After the liquid Bi is cooled to room temperature and completely solidified, a liquid electrode can be obtained.
[0024] The small crucible for loading solid Bi particles is a corundum crucible, and has a size of 29 mm in height, 20 mm in bottom diameter, and 41 mm in top diameter.
[0025] Furthermore, the temperature mentioned above for heating to a temperature above the melting point of Bi is specifically 300-350°C.
[0026] Furthermore, the W wire has a diameter of 1 mm and a length of 20 to 25 cm.
[0027] Furthermore, the W wire is processed by using 200-mesh coarse sandpaper to polish the entire body, and after the tungsten oxide on the surface of the W wire is completely polished, the W wire is placed in an ultrasonic cleaner for cleaning, and then placed in a drying oven for drying.
[0028] Furthermore, the method for pre-electrolysis in step (1) is to insert the three-electrode system into the molten salt respectively, connect the electrodes to a power source, and perform constant potential electrolysis for a period of time.
[0029] Furthermore, the carbon rod has a diameter of 5 mm, and the W wire has a diameter of 1 mm.
[0030] Furthermore, the constant potential specifically refers to -2.0V (vsAg / AgCl).
[0031] Furthermore, the time is 3 hours.
[0032] (2) Electrodeposition of uranium dioxide: Mix UO3 and NH4HF2 in a mass ratio of 1:5, then grind them in a mortar, put the mixture into a crucible, cover the crucible, put it into a pit furnace, react at a certain temperature for a period of time, and then take it out. The prepared UO2F2 is used as UO2 2+ The source of Bi is added to the treated molten salt, and the liquid electrode is inserted into the molten salt. After the solid Bi melts into liquid, the three-electrode system is connected to a power source for electrodeposition, where the potential is -0.4V to -0.8V (vsAg / AgCl) and the electrodeposition time is 8h.
[0033] Furthermore, the purity of UO3 and NH4HF2 is both above 99.9%.
[0034] Furthermore, the mortar is an agate mortar.
[0035] Furthermore, the crucible and the crucible cover are both made of ceramics.
[0036] Furthermore, the specific reaction temperature is 300-350°C.
[0037] Furthermore, the reaction time is 3h.
[0038] Furthermore, the three-electrode system used in the electrodeposition is: the anode is a graphite carbon rod with a diameter of 5 mm, the cathode is a liquid Bi electrode, and the reference electrode is an Ag / AgCl electrode. The liquid electrode is prepared by the above method.
[0039] The present invention has the following outstanding features and remarkable effects:
[0040] (1) The present invention uses high-temperature molten salt as a reaction medium, which can melt low-melting-point metals to obtain liquid electrodes, thereby providing an ideal electrode for electrodeposition of UO2 using liquid electrodes.
[0041] (2) The present invention uses liquid electrodes to electro-deposit dendrite-free UO2, thereby avoiding short circuit of the electrolytic cell due to dendrite formation.
[0042] (3) The present invention uses liquid electrodes, so that UO2 will not fall into the molten salt, UO2 is easy to recover, and the UO2 yield reaches 67.7%. This also ensures the multiple recycling of the molten salt. The liquid electrodes can also be recycled, and the operation is simple, the cost is low, and the pollution is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is the XRD pattern of the electrodeposition product;
[0044] Figure 2 The SEM image of the electrodeposition product and the EDS image in the red frame. DETAILED DESCRIPTION
[0045] Example 1
[0046] A method for preparing a liquid electrode comprises the following steps:
[0047] (1) Weigh 17 g of solid Bi particles into a prepared small crucible, place it in a pit furnace, and wait until the solid Bi is completely melted into liquid. Then, insert a 23 cm long W wire as an electrical conductor into the liquid Bi.
[0048] (2) Insert the W wire into the sleeve so that one end of the sleeve contacts the liquid Bi. Then take the small crucible out of the pit furnace. After the liquid Bi cools to room temperature and completely solidifies, a liquid electrode is obtained.
[0049] The method for electrodepositing UO2 using the above-mentioned liquid electrode comprises the following steps:
[0050] (1) Melting and purification of molten salt. Under an inert atmosphere, 83 g of LiCl-KCl was weighed and placed in a large crucible according to a mass ratio of 4.6:5.4. The crucible was then placed in a pit furnace. The molten salt was heated to 500 °C under an inert atmosphere and kept warm for 4 h. After the molten salt was melted, a three-electrode system was used, with W wire as the working electrode, carbon rod as the counter electrode, and Ag / AgCl as the reference electrode. The molten salt was pre-electrolyzed for 3 h at a potential of -2.0 V (vsAg / AgCl) to remove impurities in the molten salt.
[0051] (2) Electrodeposition of uranium dioxide. In an inert atmosphere, a three-electrode system was used for electrodeposition, with a liquid Bi electrode as the working electrode, a carbon rod as the counter electrode, and Ag / AgCl as the reference electrode. First, UO2F2 was used as UO2 2+ The source is added to the purified molten salt, the liquid electrode is inserted into the molten salt, and the electrode is connected to a power source for electrodeposition, wherein the potential is -0.4 V (vs Ag / AgCl) and the electrodeposition time is 8 h.
[0052] It has been determined that the UO2 prepared in this embodiment is all UO2 without dendrite formation, and none of them falls into the molten salt. The yield of the product is 67.7%.
[0053] Example 2
[0054] A method for preparing a liquid electrode comprises the following steps:
[0055] (1) Weigh 15 g of solid Bi particles into a prepared small crucible, place it in a pit furnace, and wait until the solid Bi is completely melted into liquid. Then, insert a 20 cm long W wire as an electrical conductor into the liquid Bi.
[0056] (2) Insert the W wire into the sleeve so that one end of the sleeve contacts the liquid Bi. Then take the small crucible out of the pit furnace. After the liquid Bi cools to room temperature and completely solidifies, a liquid electrode is obtained.
[0057] The method for electrodepositing UO2 using the above-mentioned liquid electrode comprises the following steps:
[0058] (1) Melting and purification of molten salt. Under an inert atmosphere, 98 g of LiCl-KCl was weighed and placed in a large crucible at a mass ratio of 4.8:5. The crucible was then placed in a pit furnace. The molten salt was heated to 512 °C under an inert atmosphere and kept warm for 4 h. After the molten salt was melted, a three-electrode system was used, with W wire as the working electrode, carbon rod as the counter electrode, and Ag / AgCl as the reference electrode. The molten salt was pre-electrolyzed for 3 h at a potential of -2.0 V (vsAg / AgCl) to remove impurities in the molten salt.
[0059] (2) Electrodeposition of uranium dioxide. In an inert atmosphere, a three-electrode system was used for electrodeposition, with a liquid Bi electrode as the working electrode, a carbon rod as the counter electrode, and Ag / AgCl as the reference electrode. First, UO2F2 was used as UO2 2+ The source is added to the purified molten salt, the liquid electrode is inserted into the molten salt, and the electrode is connected to a power source for electrodeposition, wherein the potential is -0.4 V (vsAg / AgCl) and the electrodeposition time is 8 h.
[0060] It has been determined that the UO2 prepared in this embodiment is all UO2 without dendrite generation, and none of them falls into the molten salt, and the yield of the product is 65.6%.
Claims
1. A method for electrodeposition of UO2 using a liquid electrode, characterized in that: The following steps are involved: S1: Preparation of liquid bismuth electrode: a small crucible containing an appropriate amount of Bi particles is placed in a well-type furnace. After Bi is melted, W wire is inserted as a conductor and the W wire is sheathed in a corundum sleeve for protection; S2: Molten salt melting and purification: Under an inert atmosphere, a large crucible containing LiCl-KCl eutectic salt is placed in a pit furnace. After the eutectic salt is melted, a three-electrode system is used to pre-electrolyze the molten salt to remove impurities; S3: Electrodeposition of uranium dioxide: Under inert atmosphere, add UO2F2 to the pre-electrolyzed molten salt, connect the electrodes to a power source and use a three-electrode system for electrodeposition.
2. The method for preparing UO2 by liquid electrode electrodeposition according to claim 1, characterized in that: The preparation method of the liquid electrode in step S1 is as follows: S11: Preparation of liquid bismuth electrode: Weigh a certain mass of solid Bi particles and put them into a prepared small crucible, then place it in a pit furnace and heat the temperature to above the melting point of Bi; S21: When the solid Bi is completely melted into liquid, the treated W wire is inserted into the liquid Bi as an electrical conductor, and then the crucible is taken out of the pit furnace; S31: After the liquid Bi is cooled to room temperature and completely solidified, a liquid electrode can be obtained.
3. The method for preparing UO2 by liquid electrode electrodeposition according to claim 1, characterized in that: The preparation temperature of the liquid Bi electrode in step S1 is 300-350°C.
4. A method for preparing UO2 by electrodeposition of a liquid electrode according to claim 1, 2 or 3, characterized in that: In the step S2, the purity of LiCl and KCl is 99.9%, and the mass ratio of LiCl to KCl is 4.6-4.8:5-5.
4.
5. The method for preparing UO2 by liquid electrode electrodeposition according to claim 4, characterized in that: In step S2, the melting temperature of the LiCl-KCl eutectic salt is 500±20°C.
6. The method for preparing UO2 by liquid electrode electrodeposition according to claim 4, characterized in that: The three-electrode system in step S2 includes: the anode is a spectral graphite rod, the cathode is a W wire, and the reference electrode is Ag / AgCl.
7. The method for preparing UO2 by liquid electrode electrodeposition according to claim 5, characterized in that: The pre-electrolysis conditions described in step S2 are constant potential -2.0V (vsAg / AgCl) and electrolysis time 3h.
8. The method for preparing UO2 by liquid electrode electrodeposition according to claim 7, characterized in that: The preparation method of UO2F2 described in step S3 is to mix UO3 and NH4HF2 in a mass ratio of 1:5, then grind them using an agate mortar, then put the mixture into a ceramic crucible, cover the ceramic crucible with a lid, put it into a pit furnace, react at a temperature of 300-350°C for 3 hours and then take it out.
9. The method for preparing UO2 by liquid electrode electrodeposition according to claim 8, characterized in that: In step S3, the anode and the reference electrode in the three-electrode system are consistent with the anode and the reference electrode in the three-electrode system in step 2, and the cathode is a liquid Bi electrode.
10. The preparation method according to claim 9, characterized in that: In step S2, the electrodeposition condition is a constant potential of -0.4V to -0.8V (vsAg / AgCl) and an electrodeposition time of 8h.