Preparation method of silicon carbide single crystal and silicon carbide single crystal

By growing on the silicon carbide single crystal and crystal surface, combining rotary lifting technology and stable growth surface of aluminum elements, the problem of cosolvent inclusion is solved, the quality and doping concentration of silicon carbide single crystal is improved, and the efficiency is achieved. Crystal growth.

CN118932487APending Publication Date: 2024-11-12TSINGHUA UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411346139.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing single crystal liquid phase growth method of silicon carbide, it is difficult to avoid the inclusion of the cosolvent, resulting in defects in the crystal and low doping concentration.

Method used

Grow on the seed crystal and crystal surface, the crystal growth interface is stably in contact with the liquid surface through rotary lifting technology, the growth surface and surface are stabilized by aluminum elements, the process conditions are controlled to reduce cosolvent inclusions, and through specific crystals The combination of cutting direction and transition metal element improves growth stability.

Benefits of technology

Long-term stable growth of high-quality silicon carbide single crystals is achieved, reducing the defects of cosolvent encapsulation in the crystal, and improving the P-type carrier doping concentration and crystal thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932487A_ABST
    Figure CN118932487A_ABST
Patent Text Reader

Abstract

The invention relates to a silicon carbide single crystal preparation method and a silicon carbide single crystal. According to the invention, the (1102) or (1101) surface of the seed crystal is used as a crystal growth surface, and the seed crystal is in contact with the liquid level of the silicon-transition metal element-aluminum element high-temperature solution for crystal growth, so that the interface of the silicon carbide crystal is always kept smooth in the rapid growth process, the defect of wrapping of a cosolvent in the crystal is reduced, the crystal thickness is increased, and the yield of the silicon carbide crystal is increased. And meanwhile, relatively high P-type carrier doping concentration is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon carbide crystal preparation, and in particular to a method for preparing a silicon carbide single crystal by a liquid phase method and the silicon carbide single crystal. Background Art

[0002] As a third-generation wide bandgap semiconductor, silicon carbide has a wide range of applications in various fields. Currently, the production of silicon carbide single crystal ingots usually adopts the liquid phase method or the gas phase method. The gas phase method relies on the sublimation of high-purity silicon carbide powder at a high temperature of 2200 degrees Celsius, and the sublimation atmosphere is condensed at the seed crystal at a lower temperature. The liquid phase method relies on the temperature gradient to drive the solute carbon in the solution from the high-temperature area to the seed crystal in the low-temperature area and supersaturated crystallization occurs to achieve the growth of the seed crystal. The growth of seed crystals through the gas phase method requires a higher sublimation temperature and a larger temperature gradient, resulting in greater thermal stress, which increases the micropipes and dislocation defects of the crystal, and even causes the crystal to crack. In contrast, the temperature gradient of the seed crystal growth achieved through the liquid phase method is smaller and the growth rate is slower, so theoretically it can achieve higher crystal quality.

[0003] The silicon carbide liquid phase growth method is a crystal growth technology that can easily prepare silicon carbide P-type substrates. This is because the P-type doping elements such as aluminum are mixed with the silicon-transition metal melt by alloying, and the growth interface can obtain a large concentration of doping elements such as aluminum, which can achieve hole carrier doping by replacing the silicon atoms in the silicon carbide.

[0004] For example, Patent Document 1 (CN117431634A) discloses a method for liquid phase growth of silicon carbide single crystals, which includes the following steps: placing raw materials such as Si, Cr, and Al into a graphite crucible, heating the crucible under vacuum, melting the mixed solution, and then bringing the seed crystal into contact with the liquid surface. After the growth is completed, the crystal is pulled away from the liquid surface and slowly cooled. Patent Document 1 adds a molten Al tank, and a radio frequency heating coil is provided on the outside of the crucible, and an additional graphite structure is provided inside the crucible, thereby reducing the surface low temperature area, reducing the loss of Al during long-term growth, and improving the utilization rate of raw materials.

[0005] Patent Document 1 does not mention the problem of solvent inclusion. However, for silicon carbide crystals, solvent inclusion is inevitable, especially in the mainstream (0001) silicon plane and (000 _ 1) When growing on carbon-surface seed crystals, due to slight fluctuations in crystal growth temperature and concentration conditions, steps often coalesce and develop into faceted macro-steps. When the macro-steps meet, gully-type defects are caused, which eventually lead to the formation of solvent inclusions. Summary of the invention

[0006] Problem that the invention aims to solve

[0007] In view of the above situation, it is necessary to provide a method for preparing a silicon carbide single crystal that can reduce the inclusion of co-solvents in the crystal and can obtain a silicon carbide single crystal with a higher crystal thickness and a higher P-type carrier doping concentration.

[0008] Solutions for solving problems

[0009] To solve the above problems, the inventors conducted research and found that in typical (0001) and During the long growth process of the seed crystal of the crystal face, due to the aluminum element in the high temperature solution, the crystal will eventually appear hexagonal, although (0001) and The crystal surface is full of solvent inclusions, but Face to face The surface will still be smooth, and the interior will be single crystal. The inventors found that this is because aluminum can stabilize Face to face Surface growth. Face to face During the growth process, the surface is located on the oblique side of the crystal, so its growth conditions are constantly changing. Face to face The surface can still maintain long-term stable growth, so it can be judged and The crystal plane is more thermodynamically stable and therefore less sensitive to fluctuations in growth conditions, which means and The crystal plane can grow within a wider range of process conditions, which improves the process tolerance and increases the crystal preparation yield.

[0010] Based on the above, the present invention provides a method for preparing a silicon carbide single crystal, which comprises the following steps:

[0011] Step S1: Provide Crystal face or Seed crystals on crystal faces;

[0012] Step S2: Put silicon, transition metal and aluminum as raw materials into a graphite crucible and heat them to melt the raw materials to form a mixed solution, and then Crystal face or The crystal surface contacts the liquid surface of the mixed solution, and the seed crystal is rotated and pulled to make the crystal grow;

[0013] Step S3: Pull the crystal upward so that the crystal growth interface is separated from the liquid surface, thereby obtaining a silicon carbide single crystal.

[0014] According to the preparation method described above, in step S1, a positive-axis silicon carbide crystal is bonded to a mold so that the (0001) surface of the crystal faces outward. The positive axis silicon carbide crystal is cut along a direction parallel to the (0001) plane with the mold facing downward and the included angle between the mold and the (0001) plane being 75.1 degrees to obtain a Seed crystal face.

[0015] According to the preparation method described above, in step S1, a positive-axis silicon carbide crystal is bonded to a mold so that the (0001) surface of the crystal faces outward. The positive axis silicon carbide crystal is cut in a direction parallel to the (0001) plane with the mold facing downward and the included angle between the mold and the (0001) plane being 62.2 degrees to obtain a Seed crystal face.

[0016] According to the preparation method described above, in step S2, the transition metal element is selected from one or more of chromium, titanium, iron, lanthanum, cerium, yttrium and cobalt.

[0017] According to the preparation method described above, the concentration of aluminum in the mixed solution is 4 mol.%-20 mol.%.

[0018] According to the preparation method described above, in step S2, the temperature of heating the raw material is 1800-2000° C., and the power of the heating coil is 5-12 kW.

[0019] According to the preparation method described above, in step S2, the rotation speed of the seed crystal during rotation and pulling is 50-200 rpm, and the pulling speed is 80-200 μm / h.

[0020] According to the preparation method described above, in step S2, the temperature gradient during crystal growth is 1-20°C / cm, and the crystal growth time is 30-200h.

[0021] According to the preparation method described above, in step S3, the speed of pulling the crystal upward is 800mm-1200mm / h; after the crystal growth interface is separated from the liquid surface, the coil power is linearly reduced to 0kW within 4-8 hours.

[0022] The present invention also provides a silicon carbide single crystal obtained by the above-mentioned preparation method, wherein the Al doping concentration in the silicon carbide single crystal is 5×10 19 Atom / cm 3 Up to 10 20 Atom / cm 3 .

[0023] Effects of the Invention

[0024] Through the above technical solution, the present invention achieves the following beneficial effects:

[0025] The preparation method of the present invention can stably prepare high-quality silicon carbide crystals for a long time. and The silicon carbide crystal is grown on the crystal plane, so that the interface of the silicon carbide crystal is always kept smooth during the rapid growth process, the defects of the co-solvent in the crystal are reduced, the crystal thickness is increased, and a higher P-type carrier doping concentration is obtained at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of seed crystal cutting in the method for preparing silicon carbide single crystal of the present invention.

[0027] Figure 2 It is a schematic diagram of the crystal plane orientation of the seed crystal in the method for preparing the silicon carbide single crystal of the present invention.

[0028] Figure 3 It is a schematic diagram of the apparatus for growing silicon carbide single crystal in the present invention.

[0029] Figure 4 is the silicon carbide single crystal grown in Example 1 ( _ 110 _ 2) Photographs of the crystal growth results of the crystal faces.

[0030] Figure 5 is the silicon carbide single crystal grown in Example 2 ( _ 110 _ 1) Photograph of the crystal growth results of the crystal face.

[0031] Description of Reference Numerals

[0032] 1 is the induction heating coil; 2 is the graphite holder; 3 is the graphite seed crystal rod; 4 is the silicon carbide ( _ 110 _ 1) or ( _ 110 _ 2) seed crystal; 5 is a graphite crucible; 6 is a silicon-transition metal element-aluminum element solution; 7 is a heat preservation layer. DETAILED DESCRIPTION

[0033] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.

[0034] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.

[0035] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0036] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0037] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0038] In this specification, the numerical range expressed using "numerical value A - numerical value B" means a range including the endpoint numerical values ​​A and B.

[0039] The method for preparing a silicon carbide single crystal of the present invention comprises the following steps:

[0040] Step S1: Provide Crystal face or Seed crystals on the crystal face;

[0041] Step S2: Put silicon, transition metal and aluminum as raw materials into a graphite crucible and heat them to melt the raw materials to form a mixed solution, and then Crystal face or The crystal surface contacts the liquid surface of the mixed solution, and the seed crystal is rotated and pulled to make the crystal grow;

[0042] Step S3: Pull the crystal upward so that the crystal growth interface is separated from the liquid surface, thereby obtaining a silicon carbide single crystal.

[0043] Each step is described in detail below with reference to the accompanying drawings.

[0044] Step S1

[0045] In step S1, if Figure 1 As shown, the positive axis silicon carbide crystal ( Figure 1 (shown in blue) bonded to a polymer tooling (also called a "mold", such as Figure 1 (as shown by the infrared frame in the figure), with the (0001) side of the crystal facing outward. The mold is oriented downward, and the angles between the mold and the horizontal direction (i.e., the direction parallel to the (0001) plane) (i.e., the inclination angles on both sides of the mold) are 75.1 degrees and 62.2 degrees respectively. Then, the positive axis silicon carbide crystal is cut along the direction parallel to the (0001) plane (i.e., the horizontal direction). After cutting, the obtained and The crystal with the surface is used as the seed crystal. Figure 2 The crystal plane of the seed crystal is shown in and Schematic diagram of the orientation.

[0046] Step S2

[0047] Step S2 is a silicon carbide single crystal growth step. Figure 3 Schematic diagram of the device for growing silicon carbide crystals in the present invention is shown in FIG. 1 , which includes a graphite crucible 5 , a graphite holder 2 , a graphite seed crystal rod 3 , and an insulation layer 7 and an induction heating coil 1 outside the graphite crucible 5 .

[0048] In step S2, the silicon carbide (1101) or (1102) seed crystal 4 obtained in step S1 is bonded to the graphite support 2, and connected to the water-cooled stainless steel seed crystal rod (not shown in the figure) through the graphite seed crystal rod 3. The graphite crucible 5 is placed in an induction heating single crystal furnace, and the graphite crucible 5 is wrapped with a thermal insulation layer 7. Silicon, transition metal element, and aluminum element raw materials are placed in the graphite crucible 5, and the induction heating coil 1 is used to heat and melt the raw materials to obtain a silicon-transition metal element-aluminum element high-temperature mixed solution. After all the raw materials are melted, the seed crystal is lowered to allow the seed crystal to or The surface contacts the liquid surface, and then the seed crystal is rotated and pulled up, so that or Liquid phase epitaxial growth was carried out on the surface.

[0051] In the present invention, the transition metal element used as a co-solvent can be selected from one or more of chromium, titanium, iron, lanthanum, cerium, yttrium and cobalt.

[0052] As mentioned above, aluminum is used to make and The growth of the surface is stable. In a mixed solution of silicon-transition metal element-aluminum element, the concentration of aluminum can be 4mol.%-20mol.%, for example, 6mol.%, 8mol.%, 10mol.%, 12mol.%, 15mol.%, 18mol.%, etc. In a mixed solution of silicon-transition metal element-aluminum element, the concentration of the transition metal element can be 40mol.%-60mol.%, for example, 45mol.%, 48mol.%, 50mol.%, 52mol.%, 55mol.%, 58mol.%, etc. In a mixed solution of silicon-transition metal element-aluminum element, the concentration of silicon can be 30mol.%~50mol.%, for example, 35mol.%, 38mol.%, 40mol.%, 42mol.%, 45mol.%, 48mol.%, etc.

[0053] The power of the induction heating coil 1 during heating can be 5-12kW. The temperature (i.e., growth temperature) of heating the silicon-transition metal element-aluminum element solution is 1800-2000°C, for example, 1820°C, 1850°C, 1880°C, 1900°C, 1920°C, 1950°C, 1980°C, etc.

[0054] When the seed crystal is rotated and pulled, the rotation speed may be 50-200rpm, for example, 80rpm, 100rpm, 120rpm, 150rpm, 180rpm, etc.; the pulling speed may be 80-200μm / h, for example, 90μm / h, 100μm / h, 120μm / h, 150μm / h, 180μm / h, etc.

[0055] In step S2, the growth temperature gradient can be controlled at 1-20°C / cm, for example, 5°C / cm, 8°C / cm, 10°C / cm, 12°C / cm, 15°C / cm, 18°C / cm, etc. The crystal growth time can be 30-200h, for example, 40h, 60h, 80h, 100h, 120h, 150h, 180h, etc.

[0056] Step S3

[0057] After 30-200 hours of growth, the crystal is pulled upward at a speed of 800mm-1200mm / h, so that the growth interface is separated from the liquid surface to end the crystal growth. Finally, the power of the induction heating coil is linearly reduced to 0kW within 4-8 hours, so that the crystal is slowly cooled to release stress. Thus, a silicon carbide single crystal is obtained.

[0058] The present invention also provides a silicon carbide single crystal obtained by the above preparation method, wherein the Al doping concentration in the silicon carbide single crystal is 5×10 19 Atom / cm3 Up to 10 20 Atom / cm 3 In addition, the crystal thickness of the silicon carbide single crystal of the present invention may be 2-10 mm.

[0059] Example

[0060] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0061] Embodiment 1:

[0062] Place the positive axis silicon carbide single crystal (0001) face outward, <11 _ 20> direction downward, the angle between the mold and the horizontal direction is 75.1°, the cutting direction is parallel to the (0001) plane, and the ( _ 110 _ 2) The crystal face is used as a seed crystal, and the seed crystal is bonded to the graphite holder 2, and the water-cooled stainless steel seed crystal rod is connected through the graphite seed crystal rod 3. The graphite crucible 5 is placed in an induction heating single crystal furnace, and the graphite crucible is surrounded by an insulation layer 7. Silicon, transition metal single substance chromium, and aluminum single substance raw materials are placed in the graphite crucible to prepare Si 40 Cr 50 Al 10 The solution system is heated and melted by induction heating coil 1 at 7kW power. After all the raw materials are melted, the liquid temperature reaches 1850℃, the seed crystal is lowered to contact the liquid surface, and the rotation and pulling at a speed of 50rpm begins. The growth temperature gradient is controlled at 10℃ / cm. The seed crystal is pulled at a speed of 100 microns per hour. After 40 hours of growth, the crystal is pulled upward at a speed of 1000mm / h, so that the growth interface is separated from the liquid surface and the crystal growth is ended. Finally, the power is linearly reduced to 0kW within 6 hours.

[0063] Figure 4 The silicon carbide single crystal grown in Example 1 is shown in ( _ 110 _ 2) Photographs of crystal growth results on the crystal face. Figure 4 It can be seen that the crystal surface is smooth, the steps are fine and dense, the crystal quality is high, and the polycrystalline and solution adhesion on the surface are the products of the seed crystal detaching from the liquid surface and cooling, which does not affect the internal quality of the crystal.

[0064] Embodiment 2:

[0065] Place the positive axis silicon carbide single crystal (0001) face outward, <11 _20> direction downward, the angle between the mold and the horizontal direction is 62.2°, the cutting direction is parallel to the (0001) plane, and the (1101) crystal plane is obtained after cutting as the seed crystal. The seed crystal is bonded to the graphite holder and connected to the water-cooled stainless steel seed crystal rod through the graphite seed crystal rod. The graphite crucible is placed in an induction heating single crystal furnace. The graphite crucible is wrapped with an insulation layer. Silicon, transition metal single substance chromium, and aluminum single substance raw materials are placed in the graphite crucible to prepare Si 40 Cr 50 Al 10 The coil heats and melts the raw materials at 7kW power. After all the raw materials are melted, the liquid temperature reaches 1850℃, the seed crystal is lowered to contact the liquid surface, and the rotation and pulling are started at 50rpm. The growth temperature gradient is controlled at 10℃ / cm. The seed crystal is pulled at a speed of 100 microns per hour. After 40 hours of growth, the crystal is pulled upward at a speed of 1000mm / h, so that the growth interface is separated from the liquid surface and the crystal growth is ended. Finally, the power is linearly reduced to 0kW within 6 hours.

[0066] Figure 5 The silicon carbide single crystal grown in Example 2 is shown in ( _ 110 _ 1) Photograph of the crystal growth result of the crystal face. Figure 5 It can be seen that the growth surface has fine steps and the surface presents a smooth mirror surface, which proves that the internal quality of the single crystal is high, the growth process is stable, and there is no solvent encapsulation defect.

[0067] The element content of the silicon carbide single crystals obtained in Example 1 and Example 2 was tested. The results showed that the doping concentration of aluminum element was 7×10 19 Atom / cm 3 and 10 20 Atom / cm 3 It can be seen that the P-type carrier concentration caused by aluminum doping is higher.

[0068] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a silicon carbide single crystal, It is characterized in that The following steps are involved: Step S1: Provide ( _ 110 _ 2) Crystal plane or ( _ 110 _ 1) Seed crystal on the crystal surface; Step S2: Put the raw materials of silicon, transition metal and aluminum into a graphite crucible and add ____ Heat is applied to melt the raw materials to form a mixed solution, then the (1102) crystal plane or the (1101) crystal plane of the seed crystal is brought into contact with the liquid surface of the mixed solution, and the seed crystal is rotated and pulled to grow a crystal; Step S3: Pull the crystal upward so that the crystal growth interface is separated from the liquid surface, thereby obtaining a silicon carbide single crystal.

2. The preparation method according to claim 1, wherein in step S1, the positive-axis silicon carbide crystal is bonded to the mold so that the (0001) surface of the crystal faces outward and the surface is less than 11 _ 20>direction downward and make the angle between the mold and the (0001) plane be 75.1 degrees, cut the positive axis silicon carbide crystal along the direction parallel to the (0001) plane, and obtain __ To a seed crystal with a (1102) crystal plane.

3. The preparation method according to claim 1, wherein in step S1, the positive-axis silicon carbide crystal is bonded to the mold so that the (0001) surface of the crystal faces outward and the surface is less than 11 _ 20>direction downward and make the angle between the mold and the (0001) plane be 62.2 degrees, cut the positive axis silicon carbide crystal along the direction parallel to the (0001) plane, and obtain __ to a seed crystal with a (1101) crystal plane.

4. The preparation method according to any one of claims 1 to 3, wherein in step S2, the transition metal element is selected from one or more of chromium, titanium, iron, lanthanum, cerium, yttrium and cobalt.

5. The preparation method according to any one of claims 1 to 4, wherein the concentration of aluminum in the mixed solution is 4 mol.% to 20 mol.%.

6. The preparation method according to any one of claims 1 to 5, wherein in step S2, the temperature of heating the raw material is 1800-2000°C, and the power of the heating coil is 5-12kW.

7. The preparation method according to any one of claims 1 to 6, wherein in step S2, the rotation speed of the seed crystal during rotational pulling is 50-200 rpm, and the pulling speed is 80-200 μm / h.

8. The preparation method according to any one of claims 1 to 7, wherein in step S2, the temperature gradient during crystal growth is 1-20°C / cm, and the crystal growth time is 30-200h.

9. The preparation method according to any one of claims 1 to 8, wherein in step S3, the speed of pulling the crystal upward is 800 mm-1200 mm / h; after the crystal growth interface is separated from the liquid surface, the coil power is linearly reduced to 0 kW within 4-8 hours.

10. A silicon carbide single crystal obtained by the preparation method according to any one of claims 1 to 9, in, The Al doping concentration in the silicon carbide single crystal is 5×10 19 Atom / cm 3 Up to 10 20 Atom / cm 3 .

Citation Information

Patent Citations

  • Silicon carbide single crystal liquid phase growth method

    CN117431634A