Texturing additive suitable for HJT slice texturing and use method thereof
By using specific combinations of velvet-making additives and process steps in HJT sheet velvet making, the problems of poor repeatability, uneven size and great environmental impact are solved, and efficient and uniform velvet-making effect and photoelectric conversion efficiency are achieved. promote.
Patent Information
- Application Number
- CN202411418653.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing HJT flake velvet additives have problems such as poor repeatability of velvet making, uneven size, poor velvet making effect under low weight reduction, great environmental impact, and the need to improve the photoelectric conversion efficiency.
It is made of suede nucleating agents, defoaming agents, auxiliary nucleating agents, surfactants, organic acids, (3,6-diaminoacridine-9-yl)boric acid, hydroxyethylhexahydrohomotriazine, The lint-making additives of stevia, amphoteric organic ion salts and water-soluble hyperbranched polyamide amines are carried out through specific formulation and process steps.
It achieves efficient, uniform and low weight reduction effect, reduces environmental pollution, improves photoelectric conversion efficiency, and is suitable for industrial production.
Smart Images

Figure CN118932496A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a texturing additive suitable for HJT thin-film texturing and a use method thereof. Background Art
[0002] HJT battery is an N-type single crystal bifacial battery, which combines the advantages of crystalline silicon battery and thin film battery, and has the advantages of high conversion efficiency, low process temperature, high stability, low attenuation rate, and bifacial power generation. It is the development direction of the new generation of battery technology. Due to the symmetrical structure + low temperature process, HJT battery is not easy to cause silicon wafer warping and is more suitable for thin-film cost reduction. Therefore, HJT thin-film texturing has become one of the important ways to reduce costs and increase efficiency of HJT batteries.
[0003] In the HJT thin-sheet texturing process, texturing additives are needed to assist. Texturing additives can not only help remove bubbles and accelerate the reaction process, but also adsorb onto the surface of the single-crystal silicon wafer as the reaction proceeds, gradually inhibiting the reaction and maintaining the texture structure. However, the existing texturing additives suitable for HJT thin-sheet texturing have more or less technical defects such as poor texturing repeatability, uneven texturing size, the texturing effect under low weight loss needs to be further improved, the texturing time is long, the impact on the environment is large, and the photovoltaic conversion efficiency of the battery needs to be further improved.
[0004] In order to solve the above technical defects, the Chinese invention patent with the authorization announcement number CN103451739B discloses a single crystal silicon wafer texturing additive, whose components include: polyethylene glycol, sodium benzoate, citric acid, hydrolyzed polymaleic anhydride, sodium acetate and the balance of water. The invention also provides a texturing liquid for single crystal silicon wafer texturing, which contains an alkaline solution and the above texturing additive, the mass ratio of the texturing additive to the alkaline solution is 0.2 to 5:100, and the alkaline solution is an aqueous solution of an inorganic base or an organic base. The invention also provides a texturing method for single crystal silicon wafers, using the above texturing liquid to texturize the surface of the single crystal silicon wafer. When the above single crystal silicon wafer texturing additive is applied to the velvet production of single crystal silicon wafers, it is not necessary to use a large amount of isopropanol or ethanol, greatly reducing the chemical oxygen demand of the texturing liquid, and can obtain uniform, small, and dense velvet pyramids, therefore, it can reduce the texturing cost, reduce environmental pollution, and is conducive to the process stability of crystalline silicon solar cells, and has good practical value. However, the velvet additive has the problem that the proportion of white spots and fingerprints on the velvet surface after velvet making is relatively high, and the velvet surface looks unclean.
[0005] It can be seen that the development of a texturing additive suitable for HJT thin-film texturing with good texturing effect and high efficiency under low weight loss, good texturing repeatability, uniform size, and environmentally friendly preparation and use process and its use method meets market demand, has broad market value and application prospects, and is of great significance to promoting the further development of the HJT battery field. Summary of the invention
[0006] The main purpose of the present invention is to provide a texturing additive suitable for HJT thin-film texturing, which has good texturing effect and high efficiency at low weight loss, good texturing repeatability, uniform size, and environmentally friendly preparation and use processes, and a method for using the same.
[0007] To achieve the above purpose, the present invention provides a texturing additive suitable for HJT thin-sheet texturing, including the following components calculated by mass percentage: 0.4wt%-1.4wt% of a texturing nucleating agent, 0.1wt%-2.1wt% of a defoaming agent, 0.2wt%-0.7wt% of an auxiliary nucleating agent, 0.2wt%-1.2wt% of a surfactant, 0.05wt%-0.2wt% of an organic acid salt, 0.01wt%-0.1wt% of (3,6-diaminoacridine-9-yl) boric acid, 0.1wt%-0.2wt% of hydroxyethyl hexahydro-s-triazine, 0.03wt%-0.12wt% of triethanolamine borate, 0.08wt%-0.15wt% of stevioside, 0.1wt%-0.2wt% of an amphoteric organic ion salt, 0.1wt%-0.3wt% of a water-soluble hyperbranched polyamide amine, and the balance being deionized water.
[0008] Preferably, the velvet nucleating agent is one or a combination of two of sodium poly(p-styrene sulfonate), polystyrene-maleic anhydride copolymer, and calcium lignin sulfonate.
[0009] Preferably, the weight average molecular weight M of the poly(sodium p-styrene sulfonate) is w =16800 g / mol,M w / M n =1.1; the polystyrene-maleic anhydride copolymer is Hua Wen ® SMA-725, maleic anhydride content is 25±2wt%, weight average molecular weight M w =100,000-140,000 g / mol.
[0010] Preferably, the defoaming agent is one or a combination of two or more of inulin, chitin, hyaluronic acid, and chondroitin sulfate.
[0011] Preferably, the auxiliary nucleating agent is one or a combination of two or more of trimethylolethane, xylitol, sorbitol and anthocyanidin.
[0012] Preferably, the surfactant is one of the nonionic surfactants PEG-2000, PEG-1000, and PEG-600, or a combination of two or more thereof.
[0013] Preferably, the organic acid salt is one of sodium benzoate, sodium propionate, and disodium succinate, or a combination of two or more thereof.
[0014] Preferably, the amphoteric organic ion salt is at least one of hydroxypropane sulfonate pyridinium salt and 1-benzylpyridine-3-carboxylate.
[0015] Preferably, there is no special requirement for the source of the water-soluble hyperbranched polyamidoamine. In one embodiment of the present invention, the water-soluble hyperbranched polyamidoamine is prepared according to the preparation method of aromatic hyperbranched polyamidoamine in Example 1 of the Chinese invention patent with authorization announcement number CN105348542B.
[0016] Another object of the present invention is to provide a method for using the texturing additive suitable for HJT thin-film texturing, comprising the following steps: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
[0017] Preferably, the mass ratio of the texturing additive to the alkali solution in step S2 is (0.35-0.6):100.
[0018] Preferably, the alkali solution in step S2 is a sodium hydroxide solution or a potassium hydroxide solution; the mass percentage concentration of the alkali solution is 0.5% to 2%.
[0019] Preferably, the front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 1% to 4%, and the mass percentage concentration of sodium hydroxide is 0.1% to 0.4%.
[0020] Preferably, the pre-cleaning temperature in step S3 is 55-65° C. and the time is 100-150 seconds.
[0021] Preferably, the texturing temperature in step S4 is 75-83° C., and the texturing time is 360-500 s.
[0022] Preferably, the alkaline solution of hydrogen peroxide in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 1-4% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.1-0.4%.
[0023] Preferably, the cleaning temperature of the hydrogen peroxide alkaline solution in step S5 is 55-65° C. and the cleaning time is 100-150 seconds.
[0024] Preferably, the acid used for the acid cleaning in step S5 is hydrofluoric acid or hydrochloric acid with a concentration of 1-3 mol / L.
[0025] Preferably, the acid cleaning in step S5 has a cleaning time of 100-200 seconds and a temperature of 25°C.
[0026] Due to the application of the above technical solution, the present invention has the following beneficial effects: (1) The method for using the texturing additive for HJT thin-sheet texturing disclosed in the present invention has a simple process, low dependence on equipment, small impact on the environment, good texturing effect, high texturing efficiency, is suitable for industrial production, and has a high value for promotion and application.
[0027] (2) The texturing additive suitable for HJT sheet texturing disclosed in the present invention includes the following components calculated by mass percentage: 0.4wt%-1.4wt% of texturing nucleating agent, 0.1wt%-2.1wt% of defoaming agent, 0.2wt%-0.7wt% of auxiliary nucleating agent, 0.2wt%-1.2wt% of surfactant, 0.05wt%-0.2wt% of organic acid salt, 0.01wt%-0.1wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.1wt%-0.2wt% of hydroxyethylhexahydrotriazine, 0.03wt%-0.12wt% of triethanolamine borate, 0.08wt%-0.15wt% of stevioside, 0.1wt%-0.2wt% of amphoteric organic ion salt, 0.1wt%-0.3wt% of water-soluble hyperbranched polyamide amine, and the balance is deionized water. Through the mutual cooperation between the components, the texturing additive suitable for HJT flake texturing has good texturing effect and high efficiency at low weight loss, good texturing repeatability and uniform size, and the preparation and use processes are environmentally friendly and suitable for HJT flake texturing.
[0028] (3) The texturing additives for HJT thin-sheet texturing disclosed in the present invention contain an electron-withdrawing group carboxyl-COONa in the organic acid salt, and a boric acid group in (3,6-diaminoacridine-9-yl)boric acid. Their combined action can accelerate the electron transfer process, thereby enhancing the corrosion of the silicon wafer by the alkali. When the molecules containing the electron-withdrawing group are adsorbed on the surface of the silicon wafer, the electrons on the surface of the silicon wafer are more easily injected from the conduction band into the solution, causing the silicon to oxidize. At the same time, due to the adsorption and desorption of the organic acid salt, the texturing nucleating agent and the auxiliary nucleating agent molecules on the surface of the silicon wafer, there is a certain rate difference in the adsorption and desorption on different crystal planes, which can reduce isotropic corrosion, and reduce the weight loss caused by excessive isotropic corrosion while ensuring the formation of the pyramid-shaped texturing surface, that is, completing the formation of the pyramid under low weight loss.
[0029] (4) The texturing additives for HJT thin-sheet texturing disclosed in the present invention, if the bubbles generated by the reaction are too large, they are easy to stay on the crystal surface, which will hinder the anisotropic reaction, increase the isotropic reaction, and then increase the etching weight loss. Through the reasonable selection of the defoaming agent and the surfactant composition, their combination can prevent the generation of large bubbles while reducing the gas-liquid-solid three-phase interfacial tension, which can effectively promote the bubbles generated by the reaction to quickly leave the silicon wafer surface, accelerate the alkali corrosion of the crystal surface, increase the anisotropy and form the velvet surface; the velvet nucleating agent used has a large molecular weight, contains more hydrocarbon groups in the molecular chain, and is more easily adsorbed on the crystal surface with a slower reaction rate, thereby reducing the consumption of alkali on the crystal surface and further accelerating the corrosion of the crystal surface. At the same time, there are also a large number of hydrophilic groups in the velvet nucleating agent, which can ensure the balance between the adsorption and desorption process of the substance on the surface, and complete the modification of the velvet surface. The addition of water-soluble hyperbranched polyamide amine can further improve the above properties and further improve the texturing effect.
[0030] (5) The texturing additive suitable for HJT thin-sheet texturing disclosed in the present invention has a texturing effect of low reflectivity, low weight loss and uniform velvet surface through reasonable selection of the composition formula, thereby solving the yield problem caused by fragments due to excessive weight loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a SEM image of the silicon wafer surface after texturing in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations. Example 1
[0033] A texturing additive suitable for HJT thin-sheet texturing comprises the following components calculated by mass percentage: 0.4wt% of a texturing nucleating agent, 0.1wt% of a defoaming agent, 0.2wt% of an auxiliary nucleating agent, 0.2wt% of a surfactant, 0.05wt% of an organic acid salt, 0.01wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.1wt% of hydroxyethylhexahydro-s-triazine, 0.03wt% of triethanolamine borate, 0.08wt% of stevioside, 0.1wt% of an amphoteric organic ion salt, 0.1wt% of a water-soluble hyperbranched polyamide amine, and the balance being deionized water.
[0034] The velvet nucleating agent is sodium poly(p-styrene sulfonate); the weight average molecular weight M of the sodium poly(p-styrene sulfonate) is w =16800 g / mol,M w / M n =1.1; the defoaming agent is inulin; the auxiliary nucleating agent is trimethylolethane; the surfactant is a nonionic surfactant PEG-2000; the organic acid salt is sodium benzoate; the amphoteric organic ion salt is hydroxypropane sulfonic acid pyridinium salt; the water-soluble hyperbranched polyamide amine is prepared according to the preparation method of the aromatic hyperbranched polyamide amine in Example 1 of the Chinese invention patent with authorization announcement number CN105348542B.
[0035] A method for using the texturing additive suitable for HJT thin-film texturing comprises the following steps: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
[0036] The mass ratio of the texturing additive to the alkali solution in step S2 is 0.35:100; the alkali solution in step S2 is a sodium hydroxide solution; and the mass percentage concentration of the alkali solution is 0.5%.
[0037] The front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 1% and the mass percentage concentration of sodium hydroxide is 0.1%.
[0038] The pre-cleaning temperature in step S3 is 55°C and the time is 100s; the texturing temperature in step S4 is 75°C and the texturing time is 360s; the hydrogen peroxide alkaline solution in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 1% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.1%.
[0039] The temperature of the hydrogen peroxide alkaline solution cleaning in step S5 is 55°C and the time is 100s; the acid used in the acid cleaning in step S5 is hydrofluoric acid with a concentration of 1 mol / L; the cleaning time of the acid cleaning in step S5 is 100s and the temperature is 25°C. Example 2
[0040] A texturing additive suitable for HJT thin-sheet texturing comprises the following components calculated by mass percentage: 0.6wt% of a texturing nucleating agent, 0.6wt% of a defoaming agent, 0.3wt% of an auxiliary nucleating agent, 0.5wt% of a surfactant, 0.1wt% of an organic acid salt, 0.03wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.13wt% of hydroxyethylhexahydro-s-triazine, 0.06wt% of triethanolamine borate, 0.1wt% of stevioside, 0.12wt% of an amphoteric organic ion salt, 0.15wt% of a water-soluble hyperbranched polyamide amine, and the balance being deionized water.
[0041] The velvet nucleating agent is polystyrene-maleic anhydride copolymer; the polystyrene-maleic anhydride copolymer is Huawen ® SMA-725, maleic anhydride content is 25±2wt%, weight average molecular weight M w =100,000 g / mol; the defoaming agent is chitin; the auxiliary nucleating agent is xylitol; the surfactant is a nonionic surfactant PEG-1000; the organic acid salt is sodium propionate; the amphoteric organic ion salt is 1-benzylpyridine-3-carboxylate; the water-soluble hyperbranched polyamide amine is prepared according to the preparation method of the aromatic hyperbranched polyamide amine in Example 1 of the Chinese invention patent with authorization announcement number CN105348542B.
[0042] A method for using the texturing additive suitable for HJT thin-film texturing comprises the following steps: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
[0043] The mass ratio of the texturing additive and the alkali solution in step S2 is 0.45:100; the alkali solution in step S2 is a potassium hydroxide solution; the mass percentage concentration of the alkali solution is 1%; the front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 2%, and the mass percentage concentration of sodium hydroxide is 0.2%.
[0044] The pre-cleaning temperature in step S3 is 57°C and the time is 120s; the texturing temperature in step S4 is 78°C and the texturing time is 400s; the hydrogen peroxide alkaline solution in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 2% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.2%.
[0045] The temperature of the hydrogen peroxide alkaline solution cleaning in step S5 is 58°C and the time is 120s; the acid used in the acid cleaning in step S5 is hydrochloric acid with a concentration of 1.5mol / L; the cleaning time of the acid cleaning in step S5 is 130s and the temperature is 25°C. Example 3
[0046] A texturing additive suitable for HJT thin-sheet texturing comprises the following components calculated by mass percentage: 0.9wt% of a texturing nucleating agent, 1.6wt% of a defoaming agent, 0.5wt% of an auxiliary nucleating agent, 0.8wt% of a surfactant, 0.13wt% of an organic acid salt, 0.06wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.15wt% of hydroxyethylhexahydro-s-triazine, 0.07wt% of triethanolamine borate, 0.12wt% of stevioside, 0.15wt% of an amphoteric organic ion salt, 0.2wt% of a water-soluble hyperbranched polyamide amine, and the balance being deionized water.
[0047] The velvet nucleating agent is calcium lignin sulfonate; the defoaming agent is hyaluronic acid; the auxiliary nucleating agent is sorbitol; the surfactant is a nonionic surfactant PEG-600; the organic acid salt is disodium succinate; the amphoteric organic ion salt is hydroxypropane sulfonic acid pyridinium salt; the water-soluble hyperbranched polyamide amine is prepared according to the preparation method of aromatic hyperbranched polyamide amine in Example 1 of the Chinese invention patent with authorization announcement number CN105348542B.
[0048] A method for using the texturing additive suitable for HJT thin-film texturing comprises the following steps: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
[0049] The mass ratio of the texturing additive and the alkali solution in step S2 is 0.5:100; the alkali solution in step S2 is a sodium hydroxide solution; the mass percentage concentration of the alkali solution is 1.3%; the front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 2.5%, and the mass percentage concentration of sodium hydroxide is 0.25%; the pre-cleaning temperature in step S3 is 60°C and the time is 130s.
[0050] The texturing temperature in step S4 is 80°C, and the texturing time is 450s; the hydrogen peroxide alkaline solution in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 3% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.3%; the hydrogen peroxide alkaline solution cleaning temperature in step S5 is 60°C, and the time is 130s; the acid used for acid cleaning in step S5 is hydrofluoric acid with a concentration of 2 mol / L; the cleaning time of the acid cleaning in step S5 is 150s, and the temperature is 25°C. Example 4
[0051] A texturing additive suitable for HJT sheet texturing, comprising the following components calculated by mass percentage: 1.3wt% of a texturing nucleating agent, 1.8wt% of a defoaming agent, 0.6wt% of an auxiliary nucleating agent, 1wt% of a surfactant, 0.17wt% of an organic acid salt, 0.09wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.18wt% of hydroxyethylhexahydro-s-triazine, 0.11wt% of triethanolamine borate, 0.13wt% of stevioside, 0.18wt% of an amphoteric organic ion salt, 0.25wt% of a water-soluble hyperbranched polyamide amine, and the balance being deionized water.
[0052] The velvet nucleating agent is a mixture of sodium poly(p-styrene sulfonate), polystyrene-maleic anhydride copolymer, and calcium lignin sulfonate in a mass ratio of 1:2:3; the weight average molecular weight M of the sodium poly(p-styrene sulfonate) is w =16800 g / mol,M w / M n = 1.1; the polystyrene-maleic anhydride copolymer is Hua Wen ® SMA-725, maleic anhydride content is 25±2wt%, weight average molecular weight M w =130,000 g / mol.
[0053] The defoaming agent is a mixture of inulin, chitin, hyaluronic acid, and chondroitin sulfate in a mass ratio of 1:2:2:1; the auxiliary nucleating agent is a mixture of trimethylolethane, xylitol, sorbitol, and anthocyanin in a mass ratio of 1:1:3:5; the surfactant is a mixture of non-ionic surfactants PEG-2000, PEG-1000, and PEG-600 in a mass ratio of 1:2:1; the organic acid salt is a mixture of sodium benzoate, sodium propionate, and disodium succinate in a mass ratio of 2:3:5; the amphoteric organic ion salt is a mixture of hydroxypropane sulfonic acid pyridinium salt and 1-benzylpyridine-3-carboxylate in a mass ratio of 1:4; the water-soluble hyperbranched polyamide amine is prepared according to the preparation method of aromatic hyperbranched polyamide amine in Example 1 of the Chinese invention patent with authorization announcement number CN105348542B.
[0054] A method for using the texturing additive suitable for HJT thin-film texturing comprises the following steps: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
[0055] The mass ratio of the texturing additive and the alkali solution in step S2 is 0.55:100; the alkali solution in step S2 is a potassium hydroxide solution; the mass percentage concentration of the alkali solution is 1.8%; the front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 3.5%, and the mass percentage concentration of sodium hydroxide is 0.35%.
[0056] The pre-cleaning temperature in step S3 is 63°C and the time is 140s; the texturing temperature in step S4 is 82°C and the texturing time is 490s; the hydrogen peroxide alkaline solution in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 3.5% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.35%; the hydrogen peroxide alkaline solution cleaning temperature in step S5 is 63°C and the time is 140s.
[0057] The acid used for the acid cleaning in step S5 is hydrochloric acid with a concentration of 2.5 mol / L; the cleaning time of the acid cleaning in step S5 is 190 s and the temperature is 25°C. Example 5
[0058] A texturing additive suitable for HJT thin-sheet texturing comprises the following components calculated by mass percentage: 1.4wt% of a texturing nucleating agent, 2.1wt% of a defoaming agent, 0.7wt% of an auxiliary nucleating agent, 1.2wt% of a surfactant, 0.2wt% of an organic acid salt, 0.1wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.2wt% of hydroxyethylhexahydro-s-triazine, 0.12wt% of triethanolamine borate, 0.15wt% of stevioside, 0.2wt% of an amphoteric organic ion salt, 0.3wt% of a water-soluble hyperbranched polyamide amine, and the balance being deionized water.
[0059] The velvet nucleating agent is calcium lignin sulfonate; the defoaming agent is chondroitin sulfate; the auxiliary nucleating agent is anthocyanin; the surfactant is a nonionic surfactant PEG-2000; the organic acid salt is sodium benzoate; the amphoteric organic ion salt is hydroxypropane sulfonic acid pyridinium salt; the water-soluble hyperbranched polyamide amine is prepared according to the preparation method of aromatic hyperbranched polyamide amine in Example 1 of the Chinese invention patent with authorization announcement number CN105348542B.
[0060] A method for using the texturing additive suitable for HJT thin-film texturing comprises the following steps: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
[0061] The mass ratio of the texturing additive to the alkali solution in step S2 is 0.6:100; the alkali solution in step S2 is a sodium hydroxide solution; and the mass percentage concentration of the alkali solution is 2%.
[0062] The front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 4% and the mass percentage concentration of sodium hydroxide is 0.4%; the pre-cleaning temperature in step S3 is 65° C. and the time is 150s.
[0063] The texturing temperature in step S4 is 83°C, and the texturing time is 500s; the hydrogen peroxide alkaline solution in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 4% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.4%; the hydrogen peroxide alkaline solution cleaning temperature in step S5 is 65°C, and the time is 150s; the acid used for acid cleaning in step S5 is hydrofluoric acid with a concentration of 3 mol / L; the cleaning time of the acid cleaning in step S5 is 200s, and the temperature is 25°C.
[0064] Comparative Example 1 The present invention provides a texturing additive suitable for HJT thin-sheet texturing and a method of using the same, which is similar to Example 1, except that no organic acid salt, triethanolamine borate and (3,6-diaminoacridine-9-yl)boric acid are added.
[0065] Comparative Example 2 The present invention provides a texturing additive suitable for HJT thin-sheet texturing and a method of using the same, which is similar to Example 1, except that hydroxyethyl hexahydro-s-triazine, stevioside and water-soluble hyperbranched polyamide amine are not added.
[0066] The texturing additives suitable for HJT thin-film texturing involved in the above Examples 1-5 and Comparative Examples 1-2 were subjected to relevant performance tests. The test results are shown in Table 1. The test method is as follows: Using a NXT Helios-rc reflectivity tester, the reflectivities obtained by testing the front and back sides of the silicon wafer respectively were taken as the average reflectivity; at the same time, the weight loss after texturing was counted and calculated.
[0067] At the same time, taking Example 1 as an example, the surface of the silicon wafer after the texturing treatment was observed using a scanning electron microscope. Figure 1 ,from Figure 1 It can be seen that the velvet surface has good uniformity, which is very helpful for the application of HJT thin-film single-crystalline silicon velvet production.
[0068] Table 1
[0069] As can be seen from Table 1, the texturing additive suitable for HJT thin-sheet texturing disclosed in the embodiment of the present invention has a more excellent texturing effect of low weight loss and low reflectivity compared with the comparative product; the addition of organic acid salts, triethanolamine borate, (3,6-diaminoacridine-9-yl) boric acid, hydroxyethyl hexahydrotriazine, stevioside and water-soluble hyperbranched polyamide amine is beneficial to improving the above properties.
[0070] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A texturing additive suitable for HJT flaking texturing, characterized in that: The invention comprises the following components calculated by mass percentage: 0.4wt%-1.4wt% of velvet nucleating agent, 0.1wt%-2.1wt% of defoaming agent, 0.2wt%-0.7wt% of auxiliary nucleating agent, 0.2wt%-1.2wt% of surfactant, 0.05wt%-0.2wt% of organic acid salt, 0.01wt%-0.1wt% of (3,6-diaminoacridine-9-yl)boric acid, 0.1wt%-0.2wt% of hydroxyethylhexahydro-s-triazine, 0.03wt%-0.12wt% of triethanolamine borate, 0.08wt%-0.15wt% of stevioside, 0.1wt%-0.2wt% of amphoteric organic ion salt, 0.1wt%-0.3wt% of water-soluble hyperbranched polyamide amine, and the balance is deionized water.
2. The texturing additive suitable for HJT flaking texturing according to claim 1, characterized in that: The velvet nucleating agent is one or a combination of two of polysodium p-styrene sulfonate, polystyrene-maleic anhydride copolymer and calcium lignin sulfonate.
3. The texturing additive suitable for HJT flaking texturing according to claim 2, characterized in that: The weight average molecular weight M of the poly(p-styrene sulfonate) w =16800 g / mol,M w / M n =1.1; the polystyrene-maleic anhydride copolymer is Hua Wen ® SMA-725, maleic anhydride content is 25±2wt%, weight average molecular weight M w =100,000-140,000 g / mol.
4. The texturing additive suitable for HJT flaking texturing according to claim 1, characterized in that: The defoaming agent is one of inulin, chitin, hyaluronic acid and chondroitin sulfate, or a combination of two or more thereof.
5. The texturing additive suitable for HJT flaking texturing according to claim 1, characterized in that: The auxiliary nucleating agent is one of trimethylolethane, xylitol, sorbitol and anthocyanin, or a combination of two or more thereof.
6. The texturing additive suitable for HJT flaking texturing according to claim 1, characterized in that: The surfactant is one of the nonionic surfactants PEG-2000, PEG-1000, and PEG-600, or a combination of two or more thereof; the organic acid salt is one of sodium benzoate, sodium propionate, and disodium succinate, or a combination of two or more thereof.
7. The texturing additive suitable for HJT flaking texturing according to claim 1, characterized in that: The amphoteric organic ion salt is at least one of hydroxypropane sulfonate pyridinium salt and 1-benzylpyridine-3-carboxylate.
8. A method for using the texturing additive for HJT lamellar texturing according to any one of claims 1 to 7, characterized in that: The steps include: Step S1, uniformly mixing the various components of the texturing additive suitable for HJT flaky texturing to obtain the texturing additive suitable for HJT flaky texturing; Step S2, adding the texturing additive suitable for HJT flake texturing prepared in step S1 into the alkali solution and stirring evenly to obtain a texturing solution; Step S3, placing the cut single crystal silicon wafer in a front hydrogen peroxide tank for pre-cleaning, and then placing it in deionized water to clean the silicon wafer; Step S4, immersing the silicon wafer processed in step S3 into a texturing solution for texturing; Step S5, sequentially wash the silicon wafer after the texturing in step S4 with deionized water, alkaline solution of hydrogen peroxide, deionized water, acid, and deionized water; then immerse it in deionized water at 85°C and slowly pull it out, and place the texturing crystalline silicon wafer in a drying oven for drying.
9. The method for using the texturing additive suitable for HJT flaking texturing according to claim 8, characterized in that: The mass ratio of the texturing additive and the alkali solution in step S2 is (0.35-0.6):100; the alkali solution in step S2 is a sodium hydroxide solution or a potassium hydroxide solution; the mass percentage concentration of the alkali solution is 0.5%-2%; the front hydrogen peroxide tank in step S3 contains a pre-prepared cleaning solution, which is a mixed aqueous solution of hydrogen peroxide and sodium hydroxide, wherein the mass percentage concentration of hydrogen peroxide is 1%-4%, and the mass percentage concentration of sodium hydroxide is 0.1%-0.4%; the pre-cleaning temperature in step S3 is 55-65°C, and the time is 100-150s.
10. The method for using the texturing additive suitable for HJT flaking texturing according to claim 8, characterized in that: The texturing temperature in step S4 is 75-83°C, and the texturing time is 360-500s; the hydrogen peroxide alkaline solution in step S5 is a mixture of a hydrogen peroxide aqueous solution with a mass percentage concentration of 1-4% and a potassium hydroxide aqueous solution with a mass percentage concentration of 0.1-0.4%; the hydrogen peroxide alkaline solution cleaning temperature in step S5 is 55-65°C, and the time is 100-150s; the acid cleaning in step S5 is hydrofluoric acid or hydrochloric acid with a concentration of 1-3mol / L; the cleaning time of the acid cleaning in step S5 is 100-200s, and the temperature is 25°C.
Citation Information
Patent Citations
Additives for texturing monocrystalline silicon wafers and their application methods
CN103451739B
Synthesis method of an aromatic hyperbranched polyamide amine
CN105348542B
A texturing liquid used for monocrystalline silicon surface texturing and a preparing method thereof
CN104120495A
Monocrystalline silicon wafer texturization liquid capable of removing peculiar smells and preparation method thereof
CN105113014A
Basket mark prevention texturing solution for HIT battery and texturing method of basket mark prevention texturing solution
CN111326410A
Cited By
Alkali-free accelerator and preparation method thereof
CN120040107A
Roughening and texturing working agent for surface treatment of semiconductor silicon-based parts and preparation method of roughening and texturing working agent
CN121802549A