Fiber membrane as well as preparation method and application thereof
By combining tetrastyrene-3,4-dihydropyrimidin-2(1H)-one with polymer and preparing fiber membranes using high-pressure electrospinning technology, the problem of slow response speed of TPE-DHPM compounds was solved, and the problem of slow response speed of TPE-DHPM compounds was achieved Fast-responsive fluorescence detection, suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202410915076.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-09
AI Technical Summary
TPE-DHPM compounds have low response speed in practical applications, and the fluorescent probe molecules have low contact efficiency with the substance to be tested, which affects their performance.
Combining tetrastyrene-3,4-dihydropyrimidine-2(1H)-one compounds with polymers to prepare fiber membranes, and preparing fiber membranes through high-pressure electrospinning technology. UV light source excitation is used to observe fluorescence changes, which is simple and efficient Acid and alkali detection is achieved.
The fiber membrane shows significant fluorescence intensity and fast acid-base environmental response. The response speed is completed within 1 second, which improves the sensitivity and accuracy of detection. It is suitable for acid-base detection, environmental monitoring, anti-counterfeiting and industrial control fields.
Smart Images

Figure CN118932533A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field related to fluorescent materials, and in particular to a fiber membrane and a preparation method and application thereof. Background Art
[0002] At the forefront of chemistry and materials science, fiber membrane materials have attracted widespread attention due to their outstanding physical and chemical properties. Due to their unique structural properties, such as large specific surface area and high porosity, these materials have shown broad application potential in many key fields such as filtration, separation, drug delivery, and tissue engineering. Although traditional fiber membrane materials, such as polypropylene and polytetrafluoroethylene, have won market favor with their excellent mechanical properties and chemical stability, their performance is still insufficient in certain specific application scenarios, such as chemical sensing and bioimaging. Therefore, in order to meet the growing demand for high-performance materials, the development of new fiber membrane materials with higher biological activity and specific functionality has become an urgent need in the industry.
[0003] In the field of fluorescent probe research, tetraphenylethylene (TPE) compounds have shown excellent fluorescence properties due to their unique aggregation-induced emission (AIE) characteristics. At the same time, 3,4-dihydropyrimidin-2(1H)-one (DHPM) compounds have broad application prospects in drug delivery, biocompatible materials and other fields due to their excellent biological activity and chemical stability. Considering the unique advantages of these two types of compounds, TPE-DHPM compounds formed by combining tetraphenylethylene with 3,4-dihydropyrimidin-2(1H)-one have shown great potential and research value as fluorescent probes.
[0004] However, in practical applications, when TPE-DHPM compounds are used as fluorescent probes, their response speed becomes an urgent problem to be solved. Although TPE-DHPM compounds themselves have excellent fluorescence properties, due to the existence of intermolecular interactions and diffusion limitations, the contact efficiency between the fluorescent probe molecules and the substances to be tested (such as acid and alkali vapor) is low, which directly affects its response speed.
[0005] Therefore, if TPE-DHPM compounds can be prepared into fiber membranes, it is expected to solve the above problems. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a fiber membrane that can not only generate fluorescence but also respond quickly to stimulations such as acid and alkali.
[0007] The invention also provides a method for preparing the fiber membrane.
[0008] The present invention also proposes the application of the fiber membrane.
[0009] According to one aspect of the present invention, a fiber membrane is provided. The raw materials for preparing the fiber membrane include a polymer and a tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one compound. The structural formula of the tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one compound is as follows:
[0010]
[0011] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the fiber membrane of the present invention has excellent fluorescence properties, not only with significant fluorescence intensity, but also with significant contrast changes in its fluorescence color in a very short time when the acid-base environment changes. This feature enables the fiber membrane to have extremely high sensitivity and accuracy in the field of acid-base detection. Even more striking is that the fiber membrane responds extremely quickly to acid-base environments and can react within just 1 second, providing strong technical support for real-time monitoring and rapid judgment. Therefore, in the fields of acid-base detection, environmental monitoring, anti-counterfeiting, textile testing, and industrial control that requires rapid response, the fiber membrane of the present invention has shown great potential application value and provided innovative solutions for the development of related industries.
[0012] In some embodiments of the present invention, the polymer includes at least one of cellulose acetate (CA), polystyrene (PS) and polylactic acid (PLA). The compounds of the present invention have good fluorescence stability in different polymer matrices.
[0013] In some embodiments of the present invention, the mass ratio of the polymer to 3,4-dihydropyrimidin-2(1H)-one is 1:0.01 to 0.1, such as 1:0.05.
[0014] In some embodiments of the present invention, the preparation raw material further includes a solvent, and the solvent is selected from a mixed solution of DMF (N,N-dimethylformamide) and DCM (dichloromethane).
[0015] In some embodiments of the present invention, the volume ratio of DMF to DCM is 1:1 to 3, such as 1:2.
[0016] In some embodiments of the present invention, the mass ratio of the 3,4-dihydropyrimidin-2(1H)-one to the solvent is 1:175-185, such as 1:179, 1:180, etc.
[0017] In some embodiments of the present invention, silicone oil paper is used as a grounding collector during the preparation of the fiber membrane.
[0018] According to another aspect of the present invention, a method for preparing the above-mentioned fiber membrane is provided, comprising the following steps:
[0019] Weighing tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one compounds and polymers and dissolving them in a solvent to prepare an electrospinning solution, loading the solution into a syringe, and extruding the solution through a spinneret at a speed of 0.8 to 1.2 mL / h (preferably 1.0 mL / h) to form filaments under the action of high-voltage static electricity; wherein the spinning voltage is 15 to 20 kV (preferably 17 kV), and the working distance is 11 to 15 cm (preferably 13 cm);
[0020] The structural formula of the tetraphenylethylene-3,4-dihydropyrimidin-2(1H)-one is as follows:
[0021]
[0022] In some embodiments of the present invention, silicone oil paper is used as a grounding collector during the preparation of the fiber membrane.
[0023] According to yet another aspect of the present invention, application of the fiber membrane in the field of detection or anti-counterfeiting is proposed.
[0024] In some embodiments of the present invention, the detection includes at least one of the following detection contents:
[0025] 1) Acidic substances;
[0026] 2) Damage to textiles.
[0027] In some embodiments of the present invention, the damage refers to damage caused by mechanics; preferably, the mechanics is mechanical force, more preferably including scratches and collisions.
[0028] In some embodiments of the present invention, the detection comprises the following steps: applying the detection content to the fiber membrane, irradiating the compound with an ultraviolet light source as an excitation light source, and observing fluorescence changes.
[0029] In some embodiments of the present invention, it is sufficient to apply it to the surface or inside of the product to be tested, without the need for complex operations such as photo-induced polymerization. The detection method of the present invention is easy to operate, has high detection efficiency, can realize batch fully automated detection, and has good industrial application prospects.
[0030] In some preferred embodiments of the present invention, the applying comprises at least one of coating, dipping, and fumigation. The coating, dipping, or fumigation operation allows the test content to be applied to the surface of the product to be tested, which is easy to operate.
[0031] In some preferred embodiments of the present invention, the wavelength of the ultraviolet light source is 320nm to 405nm; preferably 345nm to 385nm; more preferably 365nm.
[0032] According to the application of a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the compound of the present invention has strong fluorescence, and after being prepared into a fiber membrane, due to its larger specific surface area, it responds more quickly to external stimuli. The fiber membrane of the present invention responds quickly to acid and alkali, and the response to acid fumigation can be as low as 1 second, which has good industrial application prospects.
[0033] According to another aspect of the present invention, a stress detection method is proposed, comprising the following steps: attaching the above-mentioned fiber membrane to the surface and / or interior of a product to be detected, applying mechanical force to the product to be detected to achieve a force-induced response, irradiating the fiber membrane with an ultraviolet light source as an excitation light source, and observing changes in fluorescence intensity to detect stress changes.
[0034] According to another aspect of the present invention, the use of the above-mentioned fiber membrane in the preparation of toys, shape memory materials, impact-resistant protective materials, force sensor materials, and mechanical probe materials is proposed.
[0035] A material comprising the above-mentioned fiber membrane; wherein the material can be used to prepare at least one of the following products:
[0036] 1) Toys;
[0037] 2) Shape memory materials;
[0038] 3) Impact-resistant protective materials;
[0039] 4) Force sensor materials;
[0040] 5) Mechanical probe materials;
[0041] 6) Optical switch materials;
[0042] 7) Anti-counterfeiting materials;
[0043] 8) Flexible electronic products;
[0044] 9) Intelligent packaging materials.
[0045] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0047] Figure 1 These are SEM images of the nanofiber membrane obtained in Example 1 of the present invention: a) 5.0kX magnification image; b) 10.0kX magnification image.
[0048] Figure 2 The following are the fluorescent lamp photograph a), ultraviolet lamp photograph b), and inverted fluorescence microscope photograph c) of the PLA-TPE-DHPM micro-nano fiber membrane prepared in Example 1 of the present invention; the fluorescent lamp photograph d), ultraviolet lamp photograph e), and inverted fluorescence microscope photograph f) of the PS-TPE-DHPM micro-nano fiber membrane prepared in Example 3 of the present invention.
[0049] Figure 3 It is the PL spectrum and fluorescence photograph of the PLA-TPE-DHPM micro-nano fiber membrane prepared in the embodiment of the present invention under external stimulation.
[0050] Figure 4 This is the "AIE" pattern a) drawn with the powder of the TPE-DHPM compound in the comparative example of the present invention, and b) the picture of the PLA-TPE-DHPM micro-nano fiber membrane under external stimulation. The photo was taken under ultraviolet irradiation of 365nm. DETAILED DESCRIPTION
[0051] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. The test methods used in the embodiments are conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can be reagents and materials obtained from commercial channels. Unless otherwise specified, the same parameter in each embodiment has the same value. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limitations on the present invention.
[0052] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0053] The purchasing information of some raw materials used in the following examples and comparative examples is shown in Table 1 below:
[0054] Table 1
[0055]
[0056] The instrument information used in the following examples and comparative examples is shown in Table 2 below:
[0057] Table 2
[0058]
[0059]
[0060] The methods and main parameter information used in the test characterization process are as follows:
[0061] Compound 1 H-NMR and 13 C-NMR was measured on a Bruker AVANCE NEO500 spectrometer with deuterated chloroform as solvent and tetramethylsilane (TMS) as internal standard to test the chemical structure of the compounds.
[0062] Fluorescence spectra and UV-visible absorption spectra are used to analyze the photophysical properties of compounds. The excitation and emission slits of the fluorescence spectrum for AIE performance testing are 10nm and 15nm, and the rest are 3nm and 5nm.
[0063] The X-ray diffractometer uses CuKα (λ=0.1541 nm) as the light source, with a test voltage of 40 kV and 40 mA, to characterize the aggregated structure of the compound.
[0064] The fluorescence quantum efficiency of the compounds was tested using a combined steady-state / transient fluorescence spectrometer and a calibrated integrating sphere.
[0065] Scanning electron microscopy was used to observe the microstructure of the fiber membrane with an operating voltage of 15 kV.
[0066] TPEA can be prepared in-house (refer to the literature Iminoboronate-based peptide cyclization that responds to pH, oxidation, and small molecule modulators [J]. Journal of the American Chemical Society, 2016, 138 (7): 2098-2101. Preparation), or it can be purchased commercially with CAS number 1289218-74-1.
[0067] BTPE (3.35 g, 10 mmol) and 4-FPBA (1.5 g, 10 mmol) were added under nitrogen protection, and 20 mL of THF was added. The mixture was heated to 90 ° C until the raw material was dissolved. 0.5 mmol of TBAB and 18 mL of an aqueous solution containing 0.036 mol of potassium carbonate were added, and the mixture in the three-necked flask was stirred for 30 min. Pd(PPh3)4 (0.12 g, 0.1 mmol) was then added. The reaction was tracked by thin layer chromatography until the raw material disappeared. After cooling to room temperature, the prepared reaction solution in the three-necked flask was mixed and extracted three times with a mixed solution of water and ethyl acetate (1:3), and the organic solution was collected. After drying with anhydrous sodium sulfate, a solid product was obtained by rotary evaporation. The crude product was purified by silica gel chromatography column of a mixed solution of DCM and n-hexane (1:2) to obtain a pure solid product TPEA (3.23 g, yield 89%).
[0068]
[0069] The above operation was repeated several times, and the obtained products were mixed and used for the preparation of the products in the following examples.
[0070] The preparation process of TPE-DHPM is as follows:
[0071] TPEA (0.50 g, 1.38 mmol) was added to 30 mL of anhydrous ethanol, and heated with stirring. After TPEA was fully dissolved, anhydrous magnesium chloride (0.015 g, 0.138 mmol) and catalyst glacial acetic acid (9 mL, 30% of ethanol) were added and stirred at 78°C for 10 min. Urea (0.13 g, 2.08 mmol) and acetylacetone (0.138 g, 1.38 mmol) were added to the three-necked flask, and reacted for 24 h. Filtered with suction, the filter residue was repeatedly washed with ethanol for 3 times to obtain a white powder (0.4 g, 80%).
[0072] 1 H NMR (500MHz, Chloroform-d) δ8.01(s,1H),7.14–6.94(m,18H),5.58(d,J=2.5Hz,1H),5.32(d,J=2.8Hz,1H),2.32(s,3H),2.03(s,3H). 13 C NMR(151MHz,)δ194.35,151.93,148.13,143.11,142.23,140.61,140.24,130.77 ,130.61,127.84,127.79,126.60,126.51,126.04,109.13,53.60,30.11,19.65.
[0073] Example 1
[0074] In this example, a fiber membrane was prepared. 0.05g of tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one TPE-DHPM and 1g of polymer (PLA) obtained by the above operation were weighed and dissolved in a mixed solution of 8.95g DMF / DCM (v / v=1 / 2) to prepare an electrospinning solution. Then, the solution was loaded into a 10mL syringe and extruded from a spinneret at a speed of 1mL / h to form a filament under the action of high-voltage static electricity. Among them, the spinning voltage was 17kV, the working distance was 13cm, and silicone oil paper was used as a grounding collector.
[0075] Example 2
[0076] In this example, a fiber membrane was prepared. 0.05g of tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one TPE-DHPM and 1g of polymer (CA) obtained by the above operation were weighed and dissolved in a mixed solution of 8.95g DMF / DCM (v / v=1 / 2) to prepare an electrospinning solution. Then, the solution was loaded into a 10mL syringe and extruded from a spinneret at a speed of 1mL / h to form a filament under the action of high-voltage static electricity. Among them, the spinning voltage was 17kV, the working distance was 13cm, and silicone oil paper was used as a grounding collector.
[0077] Example 3
[0078] In this example, a fiber membrane was prepared. 0.05g of tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one TPE-DHPM and 1g of polymer (polystyrene (PS)) obtained by the above operation were weighed and dissolved in a mixed solution of 8.95g DMF / DCM (v / v=1 / 2) to prepare an electrospinning solution. Then, the solution was loaded into a 10mL syringe and extruded from a spinneret at a speed of 1mL / h to form a filament under the action of high-voltage static electricity. Among them, the spinning voltage was 17kV, the working distance was 13cm, and silicone oil paper was used as a grounding collector.
[0079] Comparative Example
[0080] This example provides a fluorescent material, which is 0.05 g of 3,4-dihydropyrimidin-2(1H)-one TPE-DHPM prepared by the above operation.
[0081] Test example
[0082] This test example tests the acid-base stimulus response performance of the fiber membrane prepared in the example and the fluorescent material in the comparative example. The specific operation is as follows:
[0083] Take the samples of the embodiment and the comparative example and carry out fumigation treatment with acid vapor (HCl) and alkali vapor (NH3) under the same conditions, and test their response time and fluorescence change. Since HCl and NH3 are both very volatile, a small amount of acid-base solution exists in a closed container at room temperature (25°C), and after a period of time, the entire container will be filled. The purpose of placing for a period of time is to allow the sample to be fully protonated or deprotonated. At 25°C, a small amount of hydrochloric acid solution or ammonia water is placed in a closed dryer (a hydrochloric acid aqueous solution is used, wherein the content of HCl is 36% to 38%; the alkaline solution uses ammonia water, wherein the content of NH3 is 25% to 28%. Take 10 to 15 ml of hydrochloric acid or ammonia solution and place it in a dryer of about 6.28 liters, wait for about 30 minutes at room temperature (about 25°C), and the container can be filled with acid or alkali vapor). After the acid vapor and ammonia vapor fill the dryer, place the sample in a culture dish and put it in the dryer, use a 365nm ultraviolet lamp to observe the fluorescence change, and record the response time.
[0084] The results showed that it takes a relatively long time for the TPE-DHPM compound to undergo acid-base stimulation tests in powder form. This is because the acid vapor first contacts the outermost layer of the powder, and it takes time to diffuse to the inner layer. After the initial TPE-DHPM powder was fumigated with hydrochloric acid vapor, its fluorescence color changed significantly: from the initial light blue fluorescence to dark blue fluorescence, and the emission wavelength also shifted from the initial 474nm to 456nm, indicating that the solid powder of TPE-DHPM has an obvious acid stimulation response. After ammonia vapor fumigation, the sample can be restored to its initial state. After the powder is fully ground and fumigated with hydrochloric acid vapor, it is irradiated under ultraviolet light (~4s), and the fluorescence color changes from green to yellow. Once the ultraviolet light is turned off, in a dark environment, after more than ten hours, the yellow fluorescence gradually fades to the original green. However, no photochromic phenomenon was observed in the Pristine powder after being fumigated with hydrochloric acid vapor.
[0085] The electron microscopy characterization results of PLA-TPE-DHPM fiber membrane are as follows Figure 1 As shown in the figure, it can be seen that the surface of the prepared composite fiber membrane is uniform and smooth, and no granular aggregates are observed, indicating that the TPE-DHPM compound has good compatibility with PLA, and the addition of the TPE-DHPM compound will not affect the spinning performance of PLA. At the same time, the micro-nano fiber membrane was prepared by compounding the TPE-DHPM compound with PS to explore the fluorescence stability of the TPE-DHPM compound in different polymers. The results showed that they all had good fluorescence stability.
[0086] like Figure 2As shown in the figure, PLA-TPE-DHPM micro-nanofiber membrane and PS-TPE-DHPM micro-nanofiber membrane emit blue fluorescence under 365nm ultraviolet light, and the inverted fluorescence microscope photo shows that the TPE-DHPM compound is evenly dispersed in PS and PLA polymers. The results show that the TPE-DHPM compound has good fluorescence stability in different polymers.
[0087] In the acid stimulation response experiment, after the PLA-TPE-DHPM micro-nanofiber membrane was fumigated with hydrochloric acid vapor for a period of time, it was irradiated with UV (~1s), and the fluorescence color changed from light blue to yellow, and the maximum emission wavelength of the fluorescence also shifted from 469nm to 565nm, a red shift of 96nm (e.g. Figure 3 The time for the micro-nano fiber membrane to produce photochromism after HCl fumigation under ultraviolet light is shortened from 4s in the ground state of the compound in Comparative Example 1 to 1s, mainly because the micro-nano fiber membrane has higher porosity and larger specific surface area. During the HCl vapor fumigation process, more HCl vapor will interact with TPE-DHPM molecules, thereby making the light response time faster.
[0088] The effects of other embodiments are similar to those of Embodiment 1, and are not shown one by one to avoid redundancy.
[0089] The photochromic properties of TPE-DHPM compounds after HCl vapor fumigation indicate that they have great application potential as optical recording materials. To verify their potential applications, the following tests were conducted:
[0090] First, the initial prototype was prepared by evenly applying pristine powder on weighing paper and then writing the word "AIE" on the paper. After HCl vapor fumigation, the word AIE was irradiated with ultraviolet light, and the fluorescence color gradually changed from light green to yellow ( Figure 4 As shown). Since the powder must be in an amorphous state, it will have photochromic properties after HCl vapor fumigation. PLA-TPE-DHPM micro-nano fiber membrane was prepared by electrospinning technology and made into a "pen" pattern, as shown Figure 4 After HCl vapor fumigation, the fluorescent color of the "pen tip" irradiated by the ultraviolet light shows yellow emission, while the "pen shaft" not irradiated by the ultraviolet light is consistent with the initial fluorescent color. Such high-sensitivity HCl vapor-induced photochromic performance has great application prospects in anti-counterfeiting and textile detection.
[0091] In summary, the present invention combines TPE-DHPM with polymers such as polylactic acid to prepare PLA-TPE-DHPM micro-nano fiber membranes, which improves the acid stimulation response speed and gives the micro-nano fiber membranes photochromic properties after acid fumigation. Studies have shown that the photochromic properties are mainly caused by the photocyclic reaction of TPE-DHPM compounds.
[0092] The embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A fiber membrane, characterized in that: The raw materials for preparing the fiber membrane include a polymer and a tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one compound, and the structural formula of the tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one compound is as follows:
2. The fiber membrane according to claim 1, characterized in that: The polymer includes at least one of cellulose acetate, polystyrene, and polylactic acid.
3. The fiber membrane according to claim 1, characterized in that: The mass ratio of the polymer to 3,4-dihydropyrimidine-2(1H)-one is 1:0.01-0.
1.
4. The fiber membrane according to claim 1, characterized in that: The raw material preparation further includes a solvent, and the solvent is selected from a mixed solution of DMF and DCM; preferably, the volume ratio of DMF to DCM is 1:1-3.
5. A method for preparing a fiber membrane, characterized in that: The steps include: Weighing tetraphenylethylene-3,4-dihydropyrimidine-2(1H)-one compounds and polymers and dissolving them in a solvent to prepare an electrospinning solution, loading the solution into a syringe, and extruding the solution through a spinneret at a speed of 0.8-1.2 mL / h to form filaments under the action of high-voltage static electricity; wherein the spinning voltage is 15-20 kV and the working distance is 11-15 cm; The structural formula of the tetraphenylethylene-3,4-dihydropyrimidin-2(1H)-one is as follows:
6. Use of the fiber membrane according to any one of claims 1 to 4 in the field of detection or anti-counterfeiting.
7. The use according to claim 6, characterized in that: The detection includes at least one of the following detection contents: 1) Acidic substances; 2) Damage to textiles.
8. A stress detection method, characterized in that: The method comprises the following steps: attaching the fiber membrane as described in any one of claims 1 to 4 to the surface and / or interior of the product to be detected, realizing force-induced response by applying mechanical force to the product to be detected, irradiating the fiber membrane with an ultraviolet light source as an excitation light source, observing changes in fluorescence intensity, and detecting stress changes.
9. Use of the fiber membrane according to any one of claims 1 to 4 in the preparation of toys, shape memory materials, impact-resistant protective materials, force sensor materials, and mechanical probe materials.
10. A material, characterized in that: Comprising the fiber membrane according to any one of claims 1 to 4; wherein the material can be used to prepare at least one of the following products: 1) Toys; 2) Shape memory materials; 3) Impact-resistant protective materials; 4) Force sensor materials; 5) Mechanical probe materials; 6) Optical switch materials; 7) Anti-counterfeiting materials; 8) Flexible electronic products; 9) Intelligent packaging materials.
Citation Information
Patent Citations
Fluorescent material and application thereof
CN114315732A
Composite fiber with aggregation-induced emission molecule and manufacturing method and application thereof
WO2018036021A1