Preparation process of ultraviolet aging-resistant and degradation-resistant polyester staple fibers for vehicles
By mixing barite mineral particles with titanium sulfate to form a nano-titanium dioxide coating layer, an ultrafine powdered ultraviolet shielding agent is produced and mixed with waste polyester bottles, the problem of poor UV shielding effect of automotive textiles is solved. , achieving efficient ultraviolet shielding and stable performance, improving the weather resistance and comfort of the fiber.
Patent Information
- Application Number
- CN202411232451.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
In the production of automotive textiles, the ultraviolet shielding effect is poor, the use performance is poor, the breathability is poor, and the nano-ultraviolet shielding agent is easily worn and loses its functionality, affecting the comfort and feel of the fiber.
Balite mineral particles are mixed with titanium sulfate to form a nanotitanium dioxide cladding layer. Ultrafine powdered ultraviolet shielding agent is prepared by high temperature calcination and grinding, and mixed with waste polyester bottles and melt extrusion through screws. Made polyester staple fibers that are resistant to UV aging and degradation.
It improves the shielding and weathering performance of fibers to ultraviolet rays, enhances the stability of UV resistance, avoids the sudden drop in UV shielding performance, and is simple and economical.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling waste polyester, and in particular relates to a process for preparing automotive-use polyester staple fibers resistant to ultraviolet aging and degradation. Background Art
[0002] Automotive textiles mainly include organic fabrics, knitted fabrics, nonwoven fabrics and fiber composite materials. Knitted fabrics have the characteristics of softness, comfort, good elasticity, strong extensibility and good air permeability, and their proportion has gradually increased in recent years. In addition to the comfort, beauty, economy and durability required by traditional textiles, automotive interior textile materials also have higher requirements in terms of safety and environmental protection such as anti-fouling, flame retardancy, anti-static, easy cleaning and sun resistance. Automotive interior textile materials will be degraded due to long-term ultraviolet radiation, heat and moisture. They do not have the good anti-ultraviolet performance of acrylic fiber, which affects the performance of polyester. At present, there are two main methods for producing fabrics with ultraviolet shielding function at home and abroad: one is to add ultraviolet shielding agent to fiber production to produce anti-ultraviolet fiber, and then use anti-ultraviolet fiber to produce fabrics to play the role of shielding and anti-ultraviolet function. However, this method has high technical requirements, complex process, high production cost, and is only suitable for the production of chemical fibers, not natural fibers. Another method is to use nano-TiO2 and nano-ZnO as UV shielding agents and use coating technology to coat the surface of the fabric. This method is simple and easy, but the nano-UV shielding agent is only attached to the surface of the fabric, and has poor washing resistance. It is easy to be worn and washed away, losing its functionality, and the comfort and feel of the fabric are reduced. In short, the UV shielding fabric produced by the current method has poor UV shielding effect, poor wearing performance, poor air permeability, and a strong chemical fiber feel. Summary of the invention
[0003] The purpose of the present invention is to provide a preparation process of automotive ultraviolet aging and degradation resistant polyester staple fibers which are simple in process and have strong anti-ultraviolet effect in view of the deficiencies in the prior art.
[0004] In order to achieve the above technical purpose, the technical solution adopted in the preparation process of the automotive-use ultraviolet resistant aging degradation polyester staple fiber of the present invention is as follows: A process for preparing automotive-use polyester staple fibers resistant to ultraviolet aging degradation comprises the following steps: S1. Mixing a mineral slurry containing barite mineral particles with titanyl sulfate, stirring continuously at a certain temperature, so that the titanyl sulfate is hydrolyzed on the surface of the barite to form a titanium dioxide coating layer, and then drying to obtain an intermediate; S2: calcining the intermediate at high temperature, depolymerizing and breaking it up, and organically modifying it during the breaking up process to obtain a powdered UV shielding agent; S3 further grinds the powdered UV shielding agent to obtain ultrafine UV shielding agent powder with a particle size of less than 0.01 um; S4 The waste polyester bottle flakes are crushed by a crusher to form flakes with a diameter of 10 to 20 mm, and then the flakes are sent to a cleaning tank for cleaning and then dried at low temperature; S5 The dried polyester flakes and ultraviolet shielding agent ultrafine powder are mixed evenly, and melted and extruded by a screw to obtain a melt, which enters a melt filter for filtration, is then transported to a spinning box, metered by a metering pump, spun by a spinneret assembly, and then cooled by side-blowing air to obtain nascent fibers, which are oiled and bundled before being wound and formed to obtain polyester staple fibers resistant to ultraviolet aging and degradation.
[0005] Preferably, in step S1, the mass ratio of barite to TiO2 is 1:1, and the solid content of the mineral slurry is 0.5-1%.
[0006] Preferably, in step S1, the hydrolysis pH value is 1-3, the hydrolysis temperature is 60-80°C, the time is 1-3h, the drying inlet temperature is 300-330°C, and the drying outlet temperature is 240-260°C.
[0007] Preferably, in step S1, the particle size of the barite mineral particles is 0.1 to 10 um.
[0008] Preferably, a dispersant is added during the mixing of the mineral slurry and titanyl sulfate in step S1, and the dispersant accounts for 0.1-0.3% of the total volume. The dispersant includes one or more of sodium polyacrylate, sodium hexametaphosphate, sodium hexadecyl sulfonate, and polyacrylamide.
[0009] Preferably, the high temperature calcination temperature in step S2 is 750-960° C. and the time is 2-3 hours.
[0010] Preferably, in step S5, the screw temperature is 270-280°C, the screw head pressure is 15Mpa, the filter mesh accuracy of the filter is 180 mesh, the filter temperature is 270-280°C, the spinning box body temperature is 280-290°C, the spinneret assembly pressure is 180bar, the spinning temperature is 285-290°C, and the side blowing temperature is 20-30°C.
[0011] Compared with the prior art, the present invention has the following beneficial effects: The ultraviolet shielding agent in the present invention is mainly made of barite mineral particles coated with nano titanium dioxide, which is used to increase the shielding performance and weather resistance of the fiber against ultraviolet light, and has high economic significance. Among them, the covering power of the ultraviolet shielding agent reaches 13.5g / m 2The oil absorption is 19.0g / 100g; the ultraviolet shielding agent ultrafine powder is evenly infiltrated into the treated polyester bottle pieces, thereby enhancing the anti-ultraviolet performance and anti-ultraviolet stability of the polyester fiber, and avoiding the problem of a sudden drop in anti-ultraviolet performance after washing; by recycling waste polyester bottles and integrating ultraviolet shielding agent ultrafine powder, the ultraviolet resistance of polyester staple fibers is enhanced, and the whole process is simple. DETAILED DESCRIPTION
[0012] The invention is further described below in conjunction with specific embodiments: A process for preparing automotive-use polyester staple fibers resistant to ultraviolet aging degradation comprises the following steps: S1. Mixing a mineral slurry containing barite mineral particles with titanyl sulfate, stirring continuously at a certain temperature, so that the titanyl sulfate is hydrolyzed on the surface of the barite to form a titanium dioxide coating layer, and then drying to obtain an intermediate; S2: calcining the intermediate at high temperature, depolymerizing and breaking it up, and organically modifying it during the breaking up process to obtain a powdered UV shielding agent; S3 further grinds the powdered UV shielding agent to obtain ultrafine UV shielding agent powder with a particle size of less than 0.01 um; S4 The waste polyester bottle flakes are crushed by a crusher to form flakes with a diameter of 10 to 20 mm, and then the flakes are sent to a cleaning tank for cleaning and then dried at low temperature; S5 The dried polyester flakes and ultraviolet shielding agent ultrafine powder are mixed evenly, and melted and extruded by a screw to obtain a melt, which enters a melt filter for filtration, is then transported to a spinning box, metered by a metering pump, spun by a spinneret assembly, and then cooled by side-blowing air to obtain nascent fibers, which are oiled and bundled before being wound and formed to obtain polyester staple fibers resistant to ultraviolet aging and degradation.
[0013] The present invention utilizes substances capable of absorbing or shielding ultraviolet rays to prepare anti-ultraviolet fibers. TiO2, ZnO2, SiO2, Al2O3, Fe403, mica, kaolin and the like all have the characteristic of shielding ultraviolet rays in the 300-400nm band. The present invention prepares ultraviolet shielding agents into micropowders and fuses the micropowders with fibers to prepare anti-ultraviolet fibers. Since the shielding agent particles have a large diameter, the spinning quality and the fabric feel will also be affected. Therefore, the ultraviolet shielding agents are ground to a particle diameter of less than 0.01um. Such ultrafine powders have a large specific surface area and a high surface energy. After being mixed with the fibers, the fibers can enhance the reflection and scattering effects of the fibers on ultraviolet rays, thereby preventing and reducing the passage of ultraviolet rays.
[0014] In the step S1, the mass ratio of barite to TiO2 is 1:1, the solid content of the mineral slurry is 0.5-1%, the hydrolysis pH is 1-3, the hydrolysis temperature is 60-80°C, the time is 1-3h, the drying inlet temperature is 300-330°C, the drying outlet temperature is 240-260°C, the particle size of the barite mineral particles is 0.1-10um, and a dispersant is added during the mixing process of the mineral slurry and titanyl sulfate, the dispersant accounts for 0.1-0.3% of the total volume, and the dispersant includes one or more of sodium polyacrylate, sodium hexametaphosphate, sodium hexadecyl sulfate, and polyacrylamide.
[0015] The high temperature calcination temperature in step S2 is 750-960°C for 2-3 hours. The intermediate is calcined at high temperature to form a rutile crystal, which is then dry ground and broken up, and a modifier is added to allow it to be better integrated with the fiber.
[0016] In step S5, the screw temperature is 270-280°C, the screw head pressure is 15Mpa, the filter screen accuracy is 180 mesh, the filter temperature is 270-280°C, the spinning box body temperature is 280-290°C, the spinneret assembly pressure is 180bar, the spinning temperature is 285-290°C, and the side blowing temperature is 20-30°C.
[0017] Embodiment 1 A process for preparing automotive-use polyester staple fibers resistant to ultraviolet aging degradation comprises the following steps: S1. Mix a mineral slurry containing barite mineral particles (solid content 0.5-1wt%) with titanyl sulfate, add a small amount of sodium polyacrylate accounting for about 1.5% of the slurry, and stir the mixture at 85°C for 4 hours to hydrolyze the titanyl sulfate on the surface of the barite to form a titanium dioxide coating layer, and then dry the mixture to obtain an intermediate, in which the mass ratio of barite to TiO2 is 1:1; S2 The intermediate is calcined at 850°C for 2.5 hours, kept warm for 2.5 hours, ground to above 325 mesh, depolymerized and dispersed, and organically modified during the dispersion process to obtain a powdered UV shielding agent; S3 further grinds the powdered UV shielding agent to obtain ultrafine UV shielding agent powder with a particle size of 8 nm; S4 The waste polyester bottle flakes are crushed by a crusher to form flakes with a diameter of 10 to 20 mm, and then the flakes are sent to a cleaning tank for cleaning and then dried at low temperature; S5 The dried polyester flakes and ultraviolet shielding agent ultrafine powder are mixed evenly, and the melt is obtained by screw melt extrusion. The melt enters the melt filter for filtration, and is transported to the spinning box after filtration. It is metered by a metering pump and spun by a spinneret assembly, and then cooled by side blowing to obtain nascent fibers. The nascent fibers are oiled and bundled before winding and forming. The screw temperature is 270-280°C, the screw head pressure is 15Mpa, the filter screen accuracy is 180 mesh, the filter temperature is 270-280°C, the spinning box body temperature is 280-290°C, the spinneret assembly pressure is 180bar, the spinning temperature is 285-290°C, and the side blowing temperature is 20-30°C to obtain polyester staple fibers resistant to ultraviolet aging and degradation.
[0018] Embodiment 2 A process for preparing automotive-use polyester staple fibers resistant to ultraviolet aging degradation comprises the following steps: S1. Mix a mineral slurry containing barite mineral particles (solid content 0.5-1wt%) with titanyl sulfate, add a small amount of sodium polyacrylate accounting for about 1.5% of the slurry, and stir the mixture at 85°C for 4 hours to hydrolyze the titanyl sulfate on the surface of the barite to form a titanium dioxide coating layer, and then dry the mixture to obtain an intermediate, in which the mass ratio of barite to TiO2 is 1:1; S2 The intermediate is calcined at 750°C for 2.5 hours, kept warm for 2.5 hours, ground to above 325 mesh, depolymerized and dispersed, and organically modified during the dispersion process to obtain a powdered UV shielding agent; S3 further grinds the powdered UV shielding agent to obtain ultrafine UV shielding agent powder with a particle size of 4 nm; S4 The waste polyester bottle flakes are crushed by a crusher to form flakes with a diameter of 10 to 20 mm, and then the flakes are sent to a cleaning tank for cleaning and then dried at low temperature; S5 The dried polyester flakes and ultraviolet shielding agent ultrafine powder are mixed evenly, and the melt is obtained by screw melt extrusion. The melt enters the melt filter for filtration, and is transported to the spinning box after filtration. It is metered by a metering pump and spun by a spinneret assembly, and then cooled by side blowing to obtain nascent fibers. The nascent fibers are oiled and bundled before winding and forming. The screw temperature is 270-280°C, the screw head pressure is 15Mpa, the filter screen accuracy is 180 mesh, the filter temperature is 270-280°C, the spinning box body temperature is 280-290°C, the spinneret assembly pressure is 180bar, the spinning temperature is 285-290°C, and the side blowing temperature is 20-30°C to obtain polyester staple fibers resistant to ultraviolet aging and degradation.
[0019] Embodiment 3 A process for preparing automotive-use polyester staple fibers resistant to ultraviolet aging degradation comprises the following steps: S1. Mix a mineral slurry containing barite mineral particles (solid content 0.5-1wt%) with titanyl sulfate, add a small amount of sodium polyacrylate accounting for about 1.5% of the slurry, and stir the mixture at 85°C for 4 hours to hydrolyze the titanyl sulfate on the surface of the barite to form a titanium dioxide coating layer, and then dry the mixture to obtain an intermediate, in which the mass ratio of barite to TiO2 is 1:1; S2 The intermediate is calcined at 950°C for 2.5 hours, kept warm for 2.5 hours, ground to above 325 mesh, depolymerized and dispersed, and organically modified during the dispersion process to obtain a powdered UV shielding agent; S3 further grinds the powdered UV shielding agent to obtain ultrafine UV shielding agent powder with a particle size of 6 nm; S4 The waste polyester bottle flakes are crushed by a crusher to form flakes with a diameter of 10 to 20 mm, and then the flakes are sent to a cleaning tank for cleaning and then dried at low temperature; S5 The dried polyester flakes and ultraviolet shielding agent ultrafine powder are mixed evenly, and the melt is obtained by screw melt extrusion. The melt enters the melt filter for filtration, and is transported to the spinning box after filtration. It is metered by a metering pump and spun by a spinneret assembly, and then cooled by side blowing to obtain nascent fibers. The nascent fibers are oiled and bundled before winding and forming. The screw temperature is 270-280°C, the screw head pressure is 15Mpa, the filter screen accuracy is 180 mesh, the filter temperature is 270-280°C, the spinning box body temperature is 280-290°C, the spinneret assembly pressure is 180bar, the spinning temperature is 285-290°C, and the side blowing temperature is 20-30°C to obtain polyester staple fibers resistant to ultraviolet aging and degradation.
[0020] The covering power of the polyester staple fibers resistant to ultraviolet aging degradation prepared in Examples 1 to 3 of the present invention is 13.5 g / m 2 , the oil absorption is 19.0g / 100g.
[0021] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. All equivalent changes and modifications in the shape, structure, characteristics and spirit of the claims of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A process for preparing polyester staple fibers resistant to ultraviolet aging and degradation for automobiles, characterized in that: The following steps are involved: S1. Mixing a mineral slurry containing barite mineral particles with titanyl sulfate, stirring continuously at a certain temperature, so that the titanyl sulfate is hydrolyzed on the surface of the barite to form a titanium dioxide coating layer, and then drying to obtain an intermediate; S2: calcining the intermediate at high temperature, depolymerizing and breaking it up, and organically modifying it during the breaking up process to obtain a powdered UV shielding agent; S3 further grinds the powdered UV shielding agent to obtain ultrafine UV shielding agent powder with a particle size of less than 0.01 um; S4 The waste polyester bottle flakes are crushed by a crusher to form flakes with a diameter of 10 to 20 mm, and then the flakes are sent to a cleaning tank for cleaning and then dried at low temperature; S5 The dried polyester flakes and ultraviolet shielding agent ultrafine powder are mixed evenly, and melted and extruded by a screw to obtain a melt, which enters a melt filter for filtration, is then transported to a spinning box, metered by a metering pump, spun by a spinneret assembly, and then cooled by side-blowing air to obtain nascent fibers, which are oiled and bundled before being wound and formed to obtain polyester staple fibers resistant to ultraviolet aging and degradation.
2. The process for preparing the automotive-use ultraviolet resistant aging degradation polyester staple fiber according to claim 1, characterized in that: In step S1, the mass ratio of barite to TiO2 is 1:1, and the solid content of the mineral slurry is 0.5-1%.
3. The process for preparing the automotive ultraviolet resistant aging degradation polyester staple fiber according to claim 1, characterized in that: In step S1, the hydrolysis pH value is 1-3, the hydrolysis temperature is 60-80°C, the time is 1-3h, the drying inlet temperature is 300-330°C, and the drying outlet temperature is 240-260°C.
4. The process for preparing the automotive ultraviolet resistant aging degradation polyester staple fiber according to claim 1, characterized in that: In step S1, the particle size of the barite mineral particles is 0.1 to 10 um.
5. The process for preparing the automotive ultraviolet resistant aging degradation polyester staple fiber according to claim 1, characterized in that: In the step S1, a dispersant is added during the mixing of the mineral slurry and titanyl sulfate. The dispersant accounts for 0.1-0.3% of the total volume. The dispersant includes one or more of sodium polyacrylate, sodium hexametaphosphate, sodium hexadecyl sulfonate, and polyacrylamide.
6. The process for preparing the automotive ultraviolet resistant aging degradation polyester staple fiber according to claim 1, characterized in that: The high temperature calcination temperature in step S2 is 750-960° C. and the time is 2-3 hours.
7. The process for preparing the automotive ultraviolet resistant aging degradation polyester staple fiber according to claim 1, characterized in that: In step S5, the screw temperature is 270-280°C, the screw head pressure is 15Mpa, the filter screen accuracy is 180 mesh, the filter temperature is 270-280°C, the spinning box body temperature is 280-290°C, the spinneret assembly pressure is 180bar, the spinning temperature is 285-290°C, and the side blowing temperature is 20-30°C.