Layered bimetallic oxide modified carbon fiber as well as preparation method and application thereof

By building a layered bimetal oxide frame on the surface of the carbon fiber and carbonized, the problems of improving the performance and process complexity of carbon fiber absorbing materials are solved, and efficient electromagnetic wave absorption performance and simple preparation process are achieved.

CN118932699APending Publication Date: 2024-11-12NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160405.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing carbon fiber absorbing materials have limited improvements in electromagnetic wave absorption performance, and the preparation process is complex and difficult to control, resulting in unsatisfactory wave absorption performance.

Method used

By activating the carbon fibers and uniformly constructing a layered bimetal oxide frame on its surface, a three-dimensional structure is formed by hydrothermal synthesis method, and then carbonized to improve the magnetic loss ability of the material to form layered bimetal oxide modification Carbon fiber.

Benefits of technology

Improve the electromagnetic wave absorption performance of the material, solve the electromagnetic wave reflection problem caused by the high conductivity and low impedance matching of carbon fibers, realize a richer heterojunction surface and high specific surface area, enhance the multiple reflection and scattering capabilities, and the preparation process is simple, High safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005006254100000011
    Figure HDA0005006254100000011
  • Figure HDA0005006254100000012
    Figure HDA0005006254100000012
  • Figure HDA0005006254100000021
    Figure HDA0005006254100000021
Patent Text Reader

Abstract

The invention provides a layered bimetallic oxide modified carbon fiber and a preparation method and application thereof, the layered bimetallic oxide modified carbon fiber comprises a carbon fiber, and the surface of the carbon fiber is loaded with a layered bimetallic oxide. The preparation method comprises the following steps: S1, activating carbon fibers; s2, immersing the carbon fiber obtained in the S1 into a layered double-metal hydroxide precursor solution, and carrying out a hydrothermal reaction to obtain layered double-metal hydroxide coated carbon fiber; and S3, carbonizing the carbon fiber coated with the layered double-metal hydroxide under the protection of an inert atmosphere to obtain the layered double-metal oxide modified carbon fiber. The layered bimetallic oxide modified carbon fiber is good in wave absorbing effect and simple in manufacturing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wave absorbing materials, and in particular relates to a layered bimetallic oxide (LDO) modified carbon fiber and a preparation method and application thereof. Background Art

[0002] Today, the development of high-tech military equipment such as stealth fighters and drones is facing challenges due to the influence of electromagnetic radiation. In addition, the electromagnetic radiation generated by digital devices such as mobile phones, computers, and airplanes that are changing with each passing day has caused great harm to human health. Specifically, electromagnetic radiation may interfere with the normal operation of digital devices, and may also heat human cells or interfere with the inherent electromagnetic field of the human body, thereby adversely affecting human health. Therefore, it is very necessary to develop various advanced electromagnetic wave absorbing materials.

[0003] As one of the carbon-based materials, carbon fiber has attracted widespread attention in recent years due to its light weight, high conductivity, good thermal stability and other characteristics. At present, most of the research on carbon fiber at home and abroad focuses on its mechanical properties, while ignoring its potential application value in the field of electromagnetic wave absorption. Carbon fiber has many advantages as an absorbing material, but its disadvantages are also obvious. The main ones are that the loss mechanism is single and its high conductivity will lead to mismatch with the environmental impedance, thus causing excessive interface reflection, which is difficult to meet the needs of an ideal absorbing material. Therefore, it is usually necessary to add some magnetic materials as an auxiliary to improve the absorbing performance.

[0004] Patent application number 202011616696.2 discloses a carbon fiber absorbing material and a preparation method thereof, wherein the carbon fiber is first added to a strong acid for activation treatment, and a silicon carbide fiber layer covering the carbon fiber is formed on the surface of the carbon fiber by a molten salt method and an activated carbon fiber conversion method to obtain the core-shell structure carbon / silicon carbide fiber. Due to the uncontrollability of the sintering process, the uniformity of the coating is affected, so the improvement of the absorbing performance of the prepared carbon fiber absorbing material is very limited.

[0005] Patent application number 202310696132.1 discloses a method for preparing a carbon fiber absorbing material, which is to prepare ultrafine asphalt-based carbon fiber absorbing paper by selecting ultrafine asphalt-based carbon fiber, meta-aramid precipitate, and meta-aramid chopped fiber raw materials, using meta-aramid chopped fiber as support and bonding skeleton, and meta-aramid precipitate fiber as dispersed component, and through papermaking wet forming, hot pressing, enhanced bonding and other links. The preparation process used in this invention is relatively complex, difficult to operate, and difficult to control; in addition, the absorbing performance of the prepared absorbing paper is not ideal. Summary of the invention

[0006] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a layered bimetallic oxide modified carbon fiber and a preparation method and application thereof, wherein the layered bimetallic oxide modified carbon fiber has good wave absorption effect and simple manufacturing process.

[0007] The present invention is achieved through the following technical solutions:

[0008] A layered bimetallic oxide modified carbon fiber comprises carbon fiber, and the surface of the carbon fiber is loaded with layered bimetallic oxide.

[0009] Preferably, the metals in the layered bimetallic oxide are at least two of iron, cobalt, nickel, zinc, aluminum, magnesium and manganese.

[0010] Preferably, the carbon fiber is polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber or viscose-based carbon fiber.

[0011] Preferably, based on the metal in the layered bimetallic oxide, the molar mass ratio of the layered bimetallic oxide to the carbon fiber is (1-2):100.

[0012] The present invention provides a method for preparing the layered bimetallic oxide modified carbon fiber, comprising the following steps:

[0013] S1, activation treatment of carbon fiber;

[0014] S2, immersing the carbon fiber obtained in S1 into a layered double metal hydroxide precursor solution to perform a hydrothermal reaction to obtain a layered double metal hydroxide-coated carbon fiber;

[0015] S3, carbonizing the layered double metal hydroxide coated carbon fiber under the protection of an inert atmosphere to obtain a layered double metal oxide modified carbon fiber.

[0016] Preferably, the activation treatment in S1 is carried out by a gas phase oxidation method, a plasma oxidation method, a liquid phase oxidation method, an electrochemical deposition oxidation method or an anodic oxidation method.

[0017] Preferably, in S2, the preparation method of the layered double hydroxide precursor solution is: separately preparing a double metal salt aqueous solution and an alkali source aqueous solution, and mixing the double metal salt aqueous solution and the alkali source aqueous solution to obtain the layered double hydroxide precursor solution.

[0018] Preferably, in S2, the temperature of the hydrothermal reaction is 120-150° C., and the time is 12-18 h.

[0019] Preferably, in S3, the carbonization temperature is 500-800°C and the time is 3h-5h.

[0020] The present invention also provides the use of the layered bimetallic oxide modified carbon fiber as a wave absorbing material in the field of electromagnetic wave absorption.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention combines carbon fiber with excellent dielectric properties with layered bimetallic oxides, and the layered bimetallic oxides are loaded on the surface of carbon fiber, and a hierarchical structure with a carbon fiber interconnection network as a skeleton is constructed, giving the material a richer heterojunction surface, and the unique nano-layer of LDO, the higher specific surface area of ​​the nano-rod-like structure, a large number of pores and spaces will produce multiple reflections and scatterings of electromagnetic waves, which is conducive to improving the multiple reflections and scattering of electromagnetic waves, and enhancing the polarization loss capacity; at the same time, the introduction of layered bimetallic oxides improves the magnetic loss capacity of the material, and solves the problem of single dielectric loss of traditional carbon fiber wave absorption. Therefore, the carbon fiber loaded with layered bimetallic oxides in the present invention solves the problem that the incident electromagnetic wave is prone to reflection and is not easy to enter the inside of the absorbing material due to the high conductivity and low impedance matching of carbon fiber, and the unique layered structure of the layered bimetallic oxide improves the electromagnetic wave absorption performance, so that it has good electromagnetic wave absorption performance.

[0023] The preparation method of layered bimetallic oxide modified carbon fiber of the present invention firstly performs an active treatment on the surface of the carbon fiber to introduce an activated group, which has a high specific surface area and adsorption capacity and is conducive to the grafting reaction. Then, a simple and convenient hydrothermal synthesis method is adopted to functionally modify the carbon fiber using a layered double hydroxide (LDH), and a three-dimensional layered double hydroxide framework can be uniformly constructed on the fiber surface. Then, it is subjected to a carbonization treatment to anneal and become magnetic, so as to prepare a carbon fiber absorbing material with integrated structure and function. The preparation process of the method is simple and easy to operate, has low risk, and the obtained bimetallic oxide can be uniformly distributed on the fiber surface and has low cost. Compared with other composite materials of metal oxides and carbon fibers, the present invention directly hydrothermally synthesizes bimetallic hydroxides on the fiber surface and anneals to generate the corresponding bimetallic oxides, which is simpler to prepare and more conducive to the regulation of morphology. The growth morphology can be controlled by controlling the metal ion ratio of the layered bimetallic hydroxide precursor solution.

[0024] The layered bimetallic oxide modified carbon fiber of the present invention has good electromagnetic wave absorption performance and can be applied to the field of microwave absorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is a scanning electron microscope image of the carbon fiber after surface activation treatment in Comparative Example 1;

[0027] Figure 2 This is a scanning electron microscope image of the Ni-Fe LDH coated carbon fiber prepared in Example 1;

[0028] Figure 3 This is a scanning electron microscope image of the annealed Ni-Fe LDO / CF with high electromagnetic wave absorption performance prepared in Example 1;

[0029] Figure 4 This is a scanning electron microscope image of the Ni-Co LDH coated carbon fiber prepared in Example 2;

[0030] Figure 5 This is a scanning electron microscope image of the annealed Ni-Co LDO / CF with high electromagnetic wave absorption performance prepared in Example 2;

[0031] Figure 6 This is a scanning electron microscope image of the Ni-Zn LDH coated carbon fiber prepared in Example 3;

[0032] Figure 7 This is a scanning electron microscope image of the annealed Ni-Zn LDO / CF with high electromagnetic wave absorption performance prepared in Example 3;

[0033] Figure 8 The reflection loss of the annealed Ni-Fe LDO / CF with high electromagnetic wave absorption performance prepared in Example 1;

[0034] Fig. 9 The reflection loss of the annealed Ni-Co LDO / CF with high electromagnetic wave absorption performance prepared in Example 2;

[0035] Fig.10 The reflection loss of the annealed Ni-Zn LDO / CF with high electromagnetic wave absorption performance prepared in Example 3;

[0036] Fig.11 This is the reflection loss of the carbon fiber after surface activation treatment in Comparative Example 1. DETAILED DESCRIPTION

[0037] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0038] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0039] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0040] The layered bimetallic oxide modified carbon fiber provided by the present invention comprises carbon fiber, and the surface of the carbon fiber is loaded with layered bimetallic oxide.

[0041] Wherein, the carbon fiber is polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber or viscose-based carbon fiber. The metal in the layered bimetallic oxide is any two of iron, cobalt, nickel, zinc, aluminum, magnesium and manganese. The layered bimetallic oxide is preferably Ni-Fe LDO, Ni-Co LDO or Ni-Zn LDO.

[0042] The method for preparing the layered bimetallic oxide modified carbon fiber of the present invention comprises the following steps:

[0043] Step 1, performing activation treatment on unsized or desized carbon fiber: after cleaning impurities on the surface of the carbon fiber, performing activation treatment;

[0044] Step 2, preparing an LDH precursor solution, respectively preparing a corresponding bimetallic salt aqueous solution and an alkali source aqueous solution, and mixing and stirring them to obtain a fully reacted LDH precursor solution;

[0045] Step 3, immersing the carbon fiber in an LDH precursor solution and performing a hydrothermal reaction at a certain temperature, grafting a layered double metal hydroxide with a special morphology on the surface of the carbon fiber after the hydrothermal reaction, and then washing and drying to obtain LDH-coated carbon fiber;

[0046] Step 4: Carry out carbonization annealing treatment on the carbon fiber coated with LDH in a high-temperature tube furnace under the protection of an inert atmosphere to obtain a layered bimetallic oxide modified carbon fiber with electromagnetic wave absorption capability.

[0047] In step 1 of the present invention, the method used for the activation treatment of the carbon fiber is any one of gas phase oxidation, plasma oxidation, liquid phase oxidation, electrochemical deposition oxidation and anodic oxidation. The present invention preferably uses a liquid phase oxidation method, that is, a nitric acid solution with a mass concentration of 7 to 15% is used to activate the surface of the carbon fiber, the treatment temperature is 15 to 60°C, the treatment time is 0.5h to 12h, and the preferred treatment temperature is room temperature.

[0048] The specific process of preparing the LDH precursor solution in step 2 of the present invention includes: preparing a bimetallic salt aqueous solution with a concentration of 0.01 to 0.15M and an alkali source aqueous solution with a concentration of 0.03 to 0.1M, respectively, and stirring for 5 to 30 minutes, then quickly pouring the bimetallic salt aqueous solution into the alkali source aqueous solution and mixing and stirring for 5 to 30 minutes at a stirring speed of 300 to 800 rpm to obtain an LDH precursor solution; the molar ratio of the bimetallic salt to the alkali source is (1 to 8): (2 to 9).

[0049] The metals in the bimetallic salt aqueous solution include at least two of iron, cobalt, nickel, zinc, aluminum, magnesium and manganese; the bimetallic salt used is any one of nitrate, chloride and sulfate; the alkaline source reagent used is any one of urea, sodium carbonate, sodium bicarbonate, sodium hydroxide and ammonia water.

[0050] In some specific embodiments of the present invention, the bimetallic salt aqueous solution is a mixture of nickel chloride and ferric chloride, or a mixture of nickel chloride and cobalt chloride, or a mixture of nickel chloride and zinc chloride, and the alkali source aqueous solution is a urea aqueous solution. The molar ratio of nickel chloride to ferric chloride, nickel chloride to cobalt chloride, and nickel chloride to zinc chloride is (1-4):(4-1), more preferably 2:1.

[0051] In step 3 of the present invention, the activated carbon fiber is immersed in the LDH precursor solution, placed in a high temperature and high pressure reactor, and reacted at 120-150°C for 12-18 hours to obtain carbon fiber with the corresponding LDH grafted on the surface. The subsequent drying temperature is 50-150°C, and the drying time is 1-24 hours.

[0052] In step 4 of the present invention, the inert atmosphere is nitrogen or argon; the carbonization annealing treatment adopts a gradient temperature increase, from room temperature to 500-800°C at a rate of 3-15°C / min, and after the temperature reaches the set value, the temperature is kept for 3h-5h. When the selected annealing temperature is 500°C, the LDH structure loaded on the surface of the annealed carbon fiber basically maintains the original morphology and is converted into the corresponding LDO.

[0053] Comparative Example 1

[0054] (1) Activation of carbon fiber: 6k polyacrylonitrile-based carbon fiber was selected. The unsized carbon fiber was first activated by soaking it in a nitric acid solution (H2O:HNO3=2:1) ​​at room temperature for 12 hours. After activation, the carbon fiber was washed with deionized water for 3 times, and finally the carbon fiber sample was placed in a 50°C oven for 12 hours to completely remove the HNO3 remaining on the surface of the carbon fiber.

[0055] (2) Absorption performance test: A vector network analyzer (VNA, N5234A) was used to measure electromagnetic parameters in the range of 2 to 18 GHz using the coaxial method. 23 wt% of carbon fiber was mixed with paraffin to form a coaxial ring (R = 7.00 mm, R = 3.04 mm, d = 2 mm) to prepare a test sample. The minimum reflection loss RL value was -14.77 dB (1.1 mm) and the effective absorption bandwidth EAB was 3.46 GHz (1.2 mm).

[0056] Example 1

[0057] (1) Activation of carbon fiber: First, the unsized carbon fiber was immersed in a nitric acid solution (H2O:HNO3=2:1) ​​at room temperature for 12 h for activation. After activation, the carbon fiber was washed with deionized water for 3 times, and finally the carbon fiber sample was placed in a 50°C oven for 12 h to completely remove the residual HNO3 on the surface of the carbon fiber.

[0058] (2) Hydrothermal synthesis of Ni-Fe LDH-coated carbon fibers: 0.95 g NiCl2·6H2O and 0.39 g FeCl2·4H2O (molar ratio Ni:Fe=2:1) ​​were dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution A; 0.56 g urea was dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution B. Solution A was quickly added to solution B and magnetically stirred for 10 min. The resulting mixed solution and 0.3 g carbon fibers after activation were placed in a polytetrafluoroethylene reactor lining and reacted in an oven at 120°C for 12 h to graft Ni-Fe LDH on the surface of the carbon fibers. The carbon fibers were removed from the solution, repeatedly washed with deionized water, and dried in an oven at 60°C for 12 h to obtain a carbon fiber sample coated with Ni-Fe LDH with a nano-layered morphology.

[0059] (3) Carbonization treatment of Ni-Fe LDH coated carbon fiber: The Ni-Fe LDH coated carbon fiber was placed in a quartz boat and heated from room temperature to 500 °C in a tube furnace at a heating rate of 5 °C / min for 3 h under nitrogen protection. The Ni-Fe LDO modified carbon fiber (Ni-Fe LDO@CF) sample was collected.

[0060] (4) Wave absorption performance test: A vector network analyzer (VNA, N5234A) was used to measure electromagnetic parameters in the range of 2 to 18 GHz using the coaxial method. Based on the total mass of Ni-Fe LDO modified carbon fiber and paraffin, 23wt% of Ni-Fe LDO modified carbon fiber was mixed with paraffin to form a coaxial ring (R = 7.00mm, R = 3.04mm, d = 2mm) to prepare a test sample. The minimum reflection loss RL value of the Ni-Fe LDO modified carbon fiber sample was -44.46dB (1.9mm), and the maximum absorption bandwidth EAB was 3.91GHz (1.4mm).

[0061] Example 2

[0062] (1) This step is the same as step (1) of Example 1.

[0063] (2) Hydrothermal synthesis of Ni-Co LDH-coated carbon fibers: 0.47 g NiCl2·6H2O and 0.23 g CoCl2·6H2O (molar ratio Ni:Co=2:1) ​​were dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution A; 0.28 g urea was dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution B. Solution A was quickly added to solution B and stirred magnetically for 10 min. The resulting mixed solution and 0.3 g carbon fibers after activation were placed in a polytetrafluoroethylene reactor liner and reacted in an oven at 120°C for 12 h to graft Ni-Co LDH on the surface of the carbon fibers. The carbon fibers were removed from the solution, repeatedly washed with deionized water, and dried in an oven at 60°C for 12 h to obtain a Ni-Co LDH-coated carbon fiber sample with a nanorod-like morphology.

[0064] (3) This step is the same as step (3) of Example 1, except that the Ni-Fe LDH-coated carbon fiber is replaced by the Ni-CoLDH-coated carbon fiber to obtain a Ni-Co LDO modified carbon fiber (Ni-Co LDO@CF) sample.

[0065] (4) This step is the same as step (4) of Example 1, and the minimum reflection loss RL value of the Ni-Co LDO modified carbon fiber sample is obtained to be -52.7 dB (2.1 mm), and the maximum absorption bandwidth EAB is 3.84 GHz (1.4 mm).

[0066] Example 3

[0067] (1) This step is the same as step (1) of Example 1.

[0068] (2) Hydrothermal synthesis of Ni-Zn LDH coated carbon fiber: 0.47g NiCl2·6H2O and 0.13g ZnCl2·6H2O (molar ratio Ni:Zn=2:1) ​​were dissolved in 30mL deionized water and stirred at room temperature for 10min as solution A; 0.28g urea was dissolved in 30mL deionized water and stirred at room temperature for 10min as solution B. Solution A was quickly added to solution B and magnetically stirred for 10min. The resulting mixed solution and 0.3g carbon fiber after activation were placed in a polytetrafluoroethylene reactor liner and reacted in an oven at 120℃ for 12h to graft Ni-Zn LDH on the surface of the carbon fiber. The carbon fiber was taken out of the solution, repeatedly washed with deionized water, and dried in an oven at 60℃ for 12h to collect the Ni-Zn LDH coated carbon fiber sample with nano-layered morphology.

[0069] (3) This step is basically the same as step (3) of Example 1, except that the Ni-Fe LDH-coated carbon fiber is replaced by the Ni-Zn LDH-coated carbon fiber to obtain a Ni-Zn LDO modified carbon fiber (Ni-Zn LDO@CF) sample.

[0070] (4) This step is basically the same as step (4) of Example 1, except that 20 wt% of Ni-Zn LDO modified carbon fiber is mixed with paraffin to obtain a Ni-Zn LDO modified carbon fiber sample with a minimum reflection loss RL value of -68.39 dB (1.56 mm) and an effective absorption bandwidth EAB of 4.13 GHz (1.4 mm).

[0071] Example 4

[0072] (1) This step is the same as step (1) of Example 1.

[0073] (2) Hydrothermal synthesis of Ni-Fe LDH-coated carbon fibers: 0.95 g NiCl2·6H2O and 0.39 g FeCl2·4H2O (molar ratio Ni:Fe=2:1) ​​were dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution A; 0.56 g urea was dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution B. Solution A was quickly added to solution B and magnetically stirred for 10 min. The resulting mixed solution and 0.3 g carbon fibers after activation were placed in a polytetrafluoroethylene reactor lining and reacted in an oven at 150°C for 18 h to graft Ni-Fe LDH on the surface of the carbon fibers. The carbon fibers were removed from the solution, repeatedly washed with deionized water, and dried in an oven at 60°C for 12 h to obtain a carbon fiber sample coated with Ni-Fe LDH with a nano-layered morphology.

[0074] (3) Carbonization treatment of Ni-Fe LDH coated carbon fiber: The Ni-Fe LDH coated carbon fiber was placed in a quartz boat and heated from room temperature to 800 °C in a tubular furnace at a heating rate of 5 °C / min for carbonization for 5 h under nitrogen protection. The Ni-Fe LDO modified carbon fiber (Ni-Fe LDO@CF) sample was collected.

[0075] Example 5

[0076] (1) This step is the same as step (1) of Example 1.

[0077] (2) Hydrothermal synthesis of Ni-Co LDH-coated carbon fibers: 0.47 g NiCl2·6H2O and 0.23 g CoCl2·6H2O (molar ratio Ni:Co=2:1) ​​were dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution A; 0.28 g urea was dissolved in 30 mL deionized water and stirred at room temperature for 10 min as solution B. Solution A was quickly added to solution B and stirred magnetically for 10 min. The resulting mixed solution and 0.3 g carbon fibers after activation were placed in a polytetrafluoroethylene reactor liner and reacted in an oven at 150°C for 18 h to graft Ni-Co LDH on the surface of the carbon fibers. The carbon fibers were removed from the solution, repeatedly washed with deionized water, and dried in an oven at 60°C for 12 h to obtain a Ni-Co LDH-coated carbon fiber sample with a nanorod morphology.

[0078] (3) This step is the same as step (3) of Example 4, except that the Ni-Fe LDH-coated carbon fiber is replaced by the Ni-CoLDH-coated carbon fiber to obtain a Ni-Co LDO modified carbon fiber (Ni-Co LDO@CF) sample.

[0079] Example 6

[0080] (1) This step is the same as step (1) of Example 1.

[0081] (2) Hydrothermal synthesis of Ni-Zn LDH coated carbon fiber: 0.47g NiCl2·6H2O and 0.13g ZnCl2·6H2O (molar ratio Ni:Zn=2:1) ​​were dissolved in 30mL deionized water and stirred at room temperature for 10min as solution A; 0.28g urea was dissolved in 30mL deionized water and stirred at room temperature for 10min as solution B. Solution A was quickly added to solution B and magnetically stirred for 10min. The resulting mixed solution and 0.3g carbon fiber after activation were placed in a polytetrafluoroethylene reactor liner and reacted in an oven at 150℃ for 18h to graft Ni-Zn LDH on the surface of the carbon fiber. The carbon fiber was taken out of the solution, repeatedly washed with deionized water, and dried in an oven at 60℃ for 12h to collect the Ni-Zn LDH coated carbon fiber sample with nano-layered morphology.

[0082] (3) This step is basically the same as step (4) of Example 1, except that the Ni-Fe LDH-coated carbon fiber is replaced by the Ni-Zn LDH-coated carbon fiber to obtain a Ni-Zn LDO modified carbon fiber (Ni-Zn LDO@CF) sample.

[0083] Figure 1 This is a scanning electron microscope image of the carbon fiber prepared in Comparative Example 1 and subjected to surface activation treatment. It can be seen from the image that there are a large number of longitudinal grooves on the surface of the carbon fiber, which is beneficial to the subsequent LDH grafting reaction. Figure 2 This is a scanning electron microscope image of the Ni-FeLDH-coated carbon fiber prepared in Example 1. It can be seen from the image that the Ni-Fe LDH uniformly grown on the surface of the carbon fiber has the characteristics of a dense array of nanolayers, and some nano flower balls are loaded on the outside. Figure 3 This is a scanning electron microscope image of the Ni-Fe LDO / CF obtained after annealing the Ni-Fe LDH coated carbon fiber in Example 1. It can be seen from the figure that the morphology of the nanosheet layer remains basically unchanged after annealing. Figure 1 , Figure 2 , Figure 3 This indicates that the activated CF surface exhibits abundant longitudinal grooves, which are beneficial to the attachment of LDH. After the hydrothermal reaction, the LDH nanosheets grow uniformly and the surface morphology remains basically unchanged after annealing. Its high specific surface area and a large number of pores and spaces are beneficial to the multiple reflection and scattering of electromagnetic waves.

[0084] Figure 4 This is a scanning electron microscope image of the Ni-Co LDH-coated carbon fiber prepared in Example 2. It can be seen from the image that a relatively irregular nanowire array is uniformly grown on the surface of the carbon fiber. Figure 5This is a scanning electron microscope image of the Ni-Co LDO / CF obtained after annealing the Ni-Co LDH coated carbon fiber in Example 2. It can be seen from the figure that the morphology of the nanowires remains basically unchanged after annealing.

[0085] Figure 6 This is a scanning electron microscope image of the Ni-Zn LDH coated carbon fiber prepared in Example 3. It can be seen from the image that the Ni-Zn LDH uniformly grown on the surface of the carbon fiber has the characteristics of a dense array of nanolayers and is smaller and thinner than the NiFe-LDH flake layer in Example 1. Figure 7 This is a scanning electron microscope image of the Ni-Zn LDO / CF obtained after annealing the Ni-Zn LDH coated carbon fiber in Example 3. It can be seen from the image that the morphology of the nanosheet layer remains basically unchanged after annealing.

[0086] Figure 8 The reflection loss of the Ni-Fe LDO / CF prepared in Example 1 shows that the minimum reflection loss RL value is -44.46 dB (1.9 mm) and the maximum absorption bandwidth EAB is 3.91 GHz (1.4 mm).

[0087] Fig. 9 The reflection loss of the Ni-Co LDCF prepared in Example 2 shows that its minimum reflection loss RL value is -52.7 dB (2.1 mm) and its maximum absorption bandwidth EAB is 3.84 GHz (1.4 mm).

[0088] Fig.10 The reflection loss of the Ni-Zn LDO / CF prepared in Example 3 shows that its minimum reflection loss RL value is -68.39 dB (1.56 mm) and its effective absorption bandwidth EAB is 4.13 GHz (1.4 mm).

[0089] Fig.11 The reflection loss of the carbon fiber after surface activation treatment prepared in Comparative Example 1 has a minimum reflection loss RL value of -14.77 dB (1.1 mm) and an effective absorption bandwidth EAB of 3.46 GHz (1.2 mm).

[0090] By comparing the reflection loss and effective absorption bandwidth of Examples 1-3 with those of Comparative Example 1, it can be seen that the carbon fiber loaded with layered bimetallic oxides of the present invention has higher electromagnetic wave absorption performance than pure carbon fiber. This is because it solves the problem that the incident electromagnetic waves are easily reflected and difficult to enter the interior of the absorbing material due to the high conductivity and low impedance matching of the carbon fiber, and realizes the controllable and adjustable coating and thickness of the LDO three-dimensional structure on the carbon fiber surface.

[0091] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A layered bimetallic oxide modified carbon fiber, characterized in that: The invention comprises carbon fibers, the surface of which is loaded with layered bimetallic oxides.

2. The layered bimetallic oxide modified carbon fiber according to claim 1, characterized in that: The metals in the layered bimetallic oxide are at least two of iron, cobalt, nickel, zinc, aluminum, magnesium and manganese.

3. The layered bimetallic oxide modified carbon fiber according to claim 1, characterized in that: The carbon fiber is polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber or viscose-based carbon fiber.

4. The layered bimetallic oxide modified carbon fiber according to claim 1, characterized in that Calculated based on the metal in the layered bimetallic oxide, the molar mass ratio of the layered bimetallic oxide to the carbon fiber is (1-2):

100.

5. The method for preparing layered bimetallic oxide modified carbon fibers according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, activation treatment of carbon fiber; S2, immersing the carbon fiber obtained in S1 into a layered double hydroxide precursor solution to perform a hydrothermal reaction to obtain a layered double hydroxide-coated carbon fiber; S3, carbonizing the carbon fiber coated with the layered double metal hydroxide under the protection of an inert atmosphere to obtain a layered double metal oxide modified carbon fiber.

6. The method for preparing layered bimetallic oxide modified carbon fibers according to claim 5, wherein: The activation treatment method in S1 is gas phase oxidation, plasma oxidation, liquid phase oxidation, electrochemical deposition oxidation or anodic oxidation.

7. The method for preparing layered bimetallic oxide modified carbon fibers according to claim 5, wherein: In S2, the layered double hydroxide precursor solution is prepared by separately preparing a double metal salt aqueous solution and an alkali source aqueous solution, and mixing the double metal salt aqueous solution and the alkali source aqueous solution to obtain the layered double hydroxide precursor solution.

8. The method for preparing layered bimetallic oxide modified carbon fibers according to claim 5, wherein: In S2, the temperature of the hydrothermal reaction is 120-150° C., and the time is 12-18 h.

9. The method for preparing layered bimetallic oxide modified carbon fibers according to claim 5, wherein: In S3, the carbonization temperature is 500-800°C and the time is 3h-5h.

10. Use of the layered bimetallic oxide modified carbon fiber according to any one of claims 1 to 4 as an absorbing material in the field of electromagnetic wave absorption.