Sized large-tow carbon fiber, preparation method thereof and application of sized large-tow carbon fiber in reinforced rubber composite material

By pre-oxidizing, low-temperature carbonization and surface treatment of carbon fibers, combined with specific sizing agents and drying processes, the problem of poor bonding of carbon fibers and rubber matrix is ​​solved, and the adhesion and wear resistance are significantly improved. It is suitable for large tow carbon fibers. industrial production.

CN118932716APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310536587.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The interface bond between carbon fiber and rubber matrix is ​​poor and the bondability is poor. It is difficult to achieve good bonding in large tow carbon fiber applications, resulting in poor bonding in rubber materials.

Method used

Pre-sizing-pre-drying-secondary sizing-secondary sizing-secondary sizing-secondary sizing-repellent-drying' treatment was performed using pre-sizing agent containing polyvinyl alcohol and polyether polyurethane and Resorcinol formaldehyde gel latex, the contact angle is controlled at ≤35° and the surface tension is ≤80mN/m, and the sizing effect of carbon fiber is improved through thermal oil hot rollers, infrared radiation and horizontal hot air drying.

Benefits of technology

It significantly improves the adhesion between the sizing large tow carbon fiber and the rubber matrix, reaching 150N and above, and significantly improves wear resistance to at least 25,000 times. It is suitable for industrial production lines, without large-scale transformation and is low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226498270000111
    Figure BDA0004226498270000111
  • Figure BDA0004226498270000112
    Figure BDA0004226498270000112
  • Figure BDA0004226498270000122
    Figure BDA0004226498270000122
Patent Text Reader

Abstract

The invention relates to the technical field of sizing large-tow carbon fiber preparation, in particular to sizing large-tow carbon fiber, a preparation method thereof and application of the sizing large-tow carbon fiber in reinforced rubber composite materials. The method comprises the following steps: performing pre-oxidation, low-temperature carbonization, high-temperature carbonization, surface treatment, water washing, sizing and drying, and winding to obtain sized large-tow carbon fibers; carrying out pre-sizing and pre-drying on the washed carbon fiber by adopting a pre-sizing agent containing polyvinyl alcohol and polyether polyurethane; resorcinol formaldehyde latex is adopted for secondary sizing and secondary drying, and sized large-tow carbon fibers are obtained; the contact angle of the pre-sizing agent is less than or equal to 35 degrees, and the surface tension is less than or equal to 80mN / m. The pre-drying adopts heat-conducting oil hot roller drying, and the secondary drying adopts infrared radiation and horizontal hot air drying in sequence. On the premise of meeting the basic wear resistance requirement of the sizing large-tow carbon fiber, the binding force between the sizing large-tow carbon fiber and a rubber matrix can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sized large-tow carbon fiber preparation, and in particular to a sized large-tow carbon fiber and a preparation method thereof, and application of the sized large-tow carbon fiber in reinforcing rubber composite materials. Background Art

[0002] Rubber-based composites are widely used in the industrial fields of tires, drive belts, conveyor belts and high-pressure hoses because of their good mechanical properties, toughness and elasticity. Carbon fiber reinforced rubber composites are a type of rubber-based composite that is currently receiving widespread attention. However, due to the difference in performance between the two materials, there is a problem of poor interfacial bonding between carbon fiber and rubber materials. In carbon fiber reinforced resin-based composites, surface coating with sizing agents is usually used to improve interfacial bonding, but there is currently no special sizing agent suitable for carbon fiber reinforced rubber materials. Many of the actual applications of carbon fiber reinforced rubber composites are long-term and high-intensity friction conditions, so higher requirements are also placed on the process properties such as wear resistance of carbon fiber and carbon fiber reinforced rubber composites.

[0003] CN110983778A provides a sizing method for improving the wear resistance of carbon fiber, which uses a long drying process to improve the processing performance of carbon fiber, which is time-consuming, cannot be applied online, and cannot be applied to rubber substrates.

[0004] CN106957460A discloses a heat-resistant, tear-resistant and wear-resistant bushing, which uses vinyl triethoxysilane-modified silicon carbide fiber, vinyl triethoxysilane-modified carbon fiber and the like to enhance the toughness, impact resistance and tear resistance of the composite material. However, the process is relatively complicated, and the silicon carbide fiber, which plays a major role, has a high cost, which is not conducive to promotion and application.

[0005] At present, in the process of industrial carbon fiber production, the surface interface treatment method is generally used to improve the bonding problem between carbon fiber and rubber matrix, including electrochemical treatment, acid-base treatment, surface sizing, etc. The most commonly used method is to use resorcinol formaldehyde latex (hereinafter referred to as RFL emulsion) for sizing treatment. However, it is found in actual applications that due to the weak bonding ability of RFL emulsion with the carbon fiber surface, the use of RFL emulsion alone cannot effectively improve the adhesion between carbon fiber and rubber matrix after sizing. And the above schemes cannot achieve good sizing of large tow carbon fibers of 120K and above, which leads to poor bonding between the sizing carbon fiber and the rubber matrix when applied to rubber materials. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of poor interface bonding and poor adhesion between carbon fiber and rubber matrix in the prior art, and to provide a sized large tow carbon fiber and a preparation method thereof and the application of sized large tow carbon fiber in reinforced rubber composite materials. The preparation method treats polyacrylonitrile-based precursor by pre-oxidation, low-temperature carbonization, high-temperature carbonization, surface treatment and water washing, and then uses the method of "pre-sizing-pre-drying-secondary sizing-secondary drying" to size the washed carbon fiber tow in steps, and the contact angle of the pre-sizing agent is ≤35° and the surface tension is ≤80mN / m. The present invention adopts a specific pre-sizing agent combined with a specific sizing method, which can significantly improve the bonding force between the prepared sized large tow carbon fiber and the rubber matrix under the premise of meeting the basic wear resistance requirements of the sized large tow carbon fiber.

[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing sized large-tow carbon fiber, the method comprising: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding the polyacrylonitrile-based precursor to obtain the sized large-tow carbon fiber;

[0008] The sizing and drying comprises the following steps:

[0009] Step 1: pre-sizing and pre-drying the washed carbon fiber tow using a pre-sizing agent containing polyvinyl alcohol and polyether polyurethane to obtain initial carbon fiber;

[0010] Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber;

[0011] Wherein, the contact angle of the pre-sizing agent is ≤35° and the surface tension is ≤80mN / m;

[0012] The pre-drying method is heat-conducting oil hot roller drying;

[0013] The secondary drying step comprises: performing infrared radiation drying and horizontal hot air drying in sequence.

[0014] The second aspect of the present invention provides a sized large-tow carbon fiber prepared by the preparation method described in the first aspect of the present invention.

[0015] The third aspect of the present invention provides a use of the sized large-tow carbon fiber described in the second aspect of the present invention in reinforcing a rubber composite material.

[0016] Through the above technical scheme, the sized large tow carbon fiber and the preparation method thereof provided by the present invention and the application of the sized large tow carbon fiber in reinforcing rubber composite materials obtain the following beneficial effects:

[0017] (1) In the sizing process of large-tow carbon fibers, the present invention adopts a composite production process of "pre-sizing-pre-drying-secondary sizing-secondary drying", wherein the pre-drying adopts a heat-conducting oil hot roller drying method, and the secondary drying adopts infrared radiation and horizontal hot air drying production processes in sequence, and at the same time, a pre-sizing agent with a contact angle of ≤35° and a surface tension of ≤80mN / m is used, so that the surface structure and composition of the large-tow carbon fibers can be accurately controlled, and the bonding force between the sized large-tow carbon fibers and the rubber matrix can be improved. Specifically, the bonding force can reach 150N or more.

[0018] (2) The present invention introduces polyether polyurethane into the pre-sizing agent containing polyvinyl alcohol, which can promote the mutual entanglement and penetration of the multiphase interface, effectively improve the wear resistance of the sized large-tow carbon fiber, which can reach at least 25,000 times, and further improve the bonding ability between the sized large-tow carbon fiber and the rubber matrix.

[0019] (3) The method described in the present invention is applicable to the existing large-tow carbon fiber industrial production line, does not require much modification and upgrading, and has strong process adaptability; the pre-sizing agent and RFL emulsion used are low-cost and have broad industrial application prospects. DETAILED DESCRIPTION

[0020] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0021] The first aspect of the present invention provides a method for preparing sized large-tow carbon fiber, the method comprising: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding polyacrylonitrile-based precursor to obtain the sized large-tow carbon fiber;

[0022] The sizing and drying comprises the following steps:

[0023] Step 1: pre-sizing and pre-drying the washed carbon fiber tow using a pre-sizing agent containing polyvinyl alcohol and polyether polyurethane to obtain initial carbon fiber;

[0024] Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber;

[0025] Wherein, the contact angle of the pre-sizing agent is ≤35° and the surface tension is ≤80mN / m;

[0026] The pre-drying method is heat-conducting oil hot roller drying;

[0027] The secondary drying step comprises: performing infrared radiation drying and horizontal hot air drying in sequence.

[0028] In the present invention, the inventors have found that after the polyacrylonitrile-based precursor is pre-oxidized, low-temperature carbonized, high-temperature carbonized, surface treated, and washed with water, it is then sizing in steps using the method of "pre-sizing-pre-drying-secondary sizing-secondary drying". At the same time, combined with a pre-sizing agent with a contact angle of ≤35° and a surface tension of ≤80mN / m, the secondary uniform infiltration of the RFL emulsion on the carbon fiber surface can be achieved, thereby improving the bonding strength between the sized large-tow carbon fiber and the rubber matrix.

[0029] Furthermore, due to the presence of polyether polyurethane in the pre-sizing agent, the permeability and bonding force of the interface between the RFL and the large-tow carbon fiber can be further promoted, and the wear resistance of the sized large-tow carbon fiber can be effectively improved.

[0030] In the present invention, the pre-oxidation production process is carried out in an oxidation furnace with four heating temperature zones, and the temperatures of the four heating temperature zones are 0-250°C, 0-300°C, 0-300°C and 0-350°C respectively. The pre-oxidation time of each temperature zone is the same, and the total pre-oxidation time is 30-80 minutes. The draft ratios in the oxidation furnaces of each temperature zone are controlled to be 0-1.8, 0.8-1, 0.8-1 and 0.8-1 respectively.

[0031] In the present invention, the temperatures of the four heating zones, the total time of pre-oxidation and the drawing ratio are controlled to meet the above ranges, thereby achieving efficient and rapid pre-oxidation.

[0032] In the present invention, the low-temperature carbonization production process is carried out in a low-temperature carbonization furnace with five heating temperature zones, and the temperatures of the five heating temperature zones are respectively 0-700° C., 0-700° C., 0-800° C., 0-950° C. and 0-950° C. When the pre-oxidized filament bundle runs in the low-temperature carbonization furnace, the draft ratio is controlled to be 1-1.2, and the total residence time in the low-temperature carbonization furnace is 1-10 minutes to obtain low-temperature carbonized filaments.

[0033] In the present invention, the high-temperature carbonization production process is carried out in a high-temperature carbonization furnace divided into five heating temperature zones, and the temperatures of the five heating temperature zones are respectively 0-1300° C., 0-1400° C., 0-1700° C., 0-1900° C. and 0-2200° C. When the low-temperature carbonized wire runs in the high-temperature carbonization furnace, the draft ratio is controlled to be 0.6-0.95, and the total residence time in the high-temperature carbonization furnace is 1-10 minutes to obtain the high-temperature carbonized wire.

[0034] In the present invention, the surface treatment conditions include: using ammonium bicarbonate aqueous solution as electrolyte, voltage of 15-25V, electrolyte concentration of 10-30wt%, and treatment time of 50-80 seconds.

[0035] In the present invention, the water washing conditions include: washing at 40-60°C and a water flow rate of 2500-6500 L / h.

[0036] In the present invention, the winding and collecting can be carried out under a tension of 2000-4000 cN.

[0037] In the present invention, the term "large tow" refers to a large tow carbon fiber with more than 48,000 carbon fibers per bundle (abbreviated as 48K). According to a specific embodiment of the present invention, the large tow carbon fiber described in the present invention is 120K, that is, the number of carbon fibers per bundle is 120,000.

[0038] In the present invention, the preparation method of the pre-sizing agent can adopt the preparation method of the common emulsion in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0039] In the present invention, the surface tension refers to the surface tension when the material is diluted with water to a concentration of 2 wt %.

[0040] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber emulsion is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0041] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0042] According to the present invention, the contact angle of the pre-sizing agent is ≤10° and the surface tension is ≤75 mN / m.

[0043] According to the present invention, in the pre-sizing agent, the mass ratio of the polyvinyl alcohol to the polyether polyurethane is 1:0.6-0.9.

[0044] In the present invention, when the mass ratio of the polyvinyl alcohol to the polyether polyurethane satisfies the above range, the pre-sizing agent can significantly improve the bonding force between the sized large-tow carbon fibers and the rubber matrix while improving the wear resistance thereof when used.

[0045] Furthermore, in the pre-sizing agent, the mass ratio of the polyvinyl alcohol to the polyether polyurethane is 1:0.7-0.8.

[0046] In the present invention, the polyvinyl alcohol can be polyvinyl alcohol with different alcoholysis degrees, preferably partially alcoholysed polyvinyl alcohol.

[0047] According to the present invention, the alcoholysis degree of the polyvinyl alcohol is 78-99%, preferably 88-92%.

[0048] According to the present invention, the number average molecular weight of the polyvinyl alcohol is 20000-200000 g / mol, preferably 50000-150000 g / mol;

[0049] According to the present invention, the number average molecular weight of the polyether polyurethane is 800-10000 g / mol, preferably 2000-6000 g / mol.

[0050] According to the present invention, the polyether polyurethane comprises a structural unit A provided by polyisocyanate and a structural unit B provided by polyether polyol.

[0051] According to the present invention, the molar ratio of the structural unit A to the structural unit B is 1-2:1.

[0052] According to the present invention, the polyisocyanate is an aromatic polyisocyanate.

[0053] In the present invention, the polyisocyanate is selected from aromatic polyisocyanates compared to aliphatic polyisocyanates, so that the prepared polyether polyurethane can further improve the bonding force between the sized large tow carbon fiber and the rubber matrix when applied to the pre-sizing agent and used in combination with the RFL emulsion.

[0054] In the present invention, the aromatic polyisocyanate is selected from toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), polymethylene polyphenyl isocyanate (PAPI), etc., preferably at least one of toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI).

[0055] In the present invention, the polyether polyol is not particularly limited, and may be, for example, a random block polyether polyol prepared by using a polyhydroxy compound, a primary amino compound or an alcohol amine as an initiator and an epoxy compound such as propylene oxide or ethylene oxide as a polymerization monomer.

[0056] Furthermore, the polymerizable monomer is preferably ethylene oxide and / or propylene oxide.

[0057] In the present invention, the polyether polyol can be obtained commercially.

[0058] According to the present invention, in step 1, the pre-drying temperature is 60-100°C, preferably 70-90°C.

[0059] According to the present invention, the temperature of the infrared radiation drying is 65-215°C, preferably 85-165°C.

[0060] According to the present invention, the temperature of the horizontal hot air drying is 90-240°C, preferably 110-190°C.

[0061] In the present invention, the infrared radiation drying can be performed using an infrared radiation drying machine, the infrared radiation heating drying machine contains a carbon medium wave infrared radiator, and the horizontal hot air drying can be performed using a horizontal hot air drying machine.

[0062] In the present invention, when infrared radiation drying is performed, the distance between the carbon medium wave infrared radiator of the infrared radiation heating dryer and the carbon fiber is 40-180 mm, and the power density is 20-100 kW / m 2 .

[0063] According to the present invention, in the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:3-25, preferably 1:8-18.

[0064] In the present invention, based on the weight of the washed carbon fiber tow, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%.

[0065] In the present invention, based on the weight of the washed carbon fiber tow, the secondary sizing amount of the secondary sizing agent is 5-35wt%, preferably 10-20wt%.

[0066] The second aspect of the present invention provides a sized large-tow carbon fiber prepared by the preparation method described in the first aspect of the present invention.

[0067] The third aspect of the present invention provides a use of the sized large-tow carbon fiber described in the second aspect of the present invention in reinforcing a rubber composite material.

[0068] In the present invention, when the sized large-tow carbon fiber is used to prepare a reinforced rubber composite material, the content of the sized large-tow carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0069] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0070] In the present invention, the rubber material can be a rubber material commonly used in the art, for example, it can be acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, butyl rubber, etc., preferably the same type as the rubber emulsion in the RFL emulsion.

[0071] The present invention will be described in detail below by way of examples. In the following examples, each parameter is obtained by the following method.

[0072] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0073] Surface tension: The pre-sizing agent was diluted to a concentration of 2 wt % and the surface tension was tested using a dynamic surface tension meter at a temperature of 25°C.

[0074] Adhesion: The sized large tow carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sized large tow carbon fiber is 20wt% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sized large tow carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out 1 cm of length is the adhesion between the fiber and the rubber.

[0075] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0076] Abrasion times: The TM200H yarn abrasion tester is used to test the number of times the sized large-tow carbon fiber is rubbed to break.

[0077] Polyether polyurethane was purchased from Shanghai Institute of Organic Chemistry, Chinese Academy of Sciences, with the following brands: Crysol 6135, Crysol 6528, Crysol6122, Crysol 6140, Crysol 6126, Crysol 6130;

[0078] KTM-2S epoxy emulsion, purchased from Sinopharm Reagent;

[0079] Polyvinyl alcohol (PVA) was purchased from Sinopharm.

[0080] Examples 1-6

[0081] Embodiments 1-6 are methods for manufacturing a uniform 120K large-tow carbon fiber, comprising:

[0082] Pre-oxidation: The polyacrylonitrile-based precursor passes through oxidation furnace No. 1, oxidation furnace No. 2, oxidation furnace No. 3, and oxidation furnace No. 4 for pre-oxidation treatment. The temperatures of the four heating temperature zones are 238°C, 249°C, 260°C, and 270°C, respectively. The pre-oxidation time in each temperature zone is the same, and the total pre-oxidation time is 60 minutes. The draft ratios between the oxidation furnaces in the four heating temperature zones are 1.23, 0.99, 0.99, and 0.97, respectively;

[0083] Low-temperature carbonization: Using nitrogen as the medium, the pre-oxidized filament bundles were sequentially passed through a low-temperature carbonization furnace with five heating temperature zones at 515°C, 610°C, 680°C, 790°C, and 845°C, respectively. The draft ratio of each zone was controlled to be 1.08, and the total residence time in the low-temperature carbonization furnace was 1.2 minutes to obtain low-temperature carbonized filaments.

[0084] High temperature carbonization: using nitrogen as the medium, the low temperature carbonized wire is sequentially passed through a high temperature carbonization furnace with 5 heating temperature zones of 940°C, 1230°C, 1245°C, 1325°C and 1425°C, respectively, the draft ratio of each zone is controlled to be 0.79, and the total residence time in the high temperature carbonization furnace is 1.2 minutes, to obtain a high temperature carbonized wire;

[0085] Surface treatment: The high-temperature carbonized fibers are passed through a traction device into a surface treatment tank, with an ammonium bicarbonate aqueous solution as the electrolyte, a voltage of 20 V, an electrolyte concentration of 20 wt%, and a treatment time of 60 seconds to obtain surface-treated carbon fibers;

[0086] Washing: washing the surface-treated carbon fiber at a washing flow rate of 4000 L / h and a washing temperature of 54° C. to obtain a washed carbon fiber tow;

[0087] Sizing and drying: The washed carbon fiber tow is directly introduced into the first sizing tank for pre-sizing, and then passes through the heat transfer oil hot roller for pre-drying under the set process parameters; then enters the second sizing tank for secondary sizing, and then passes through the infrared radiation dryer and horizontal hot air drying in turn, and is dried again under the set process parameters to obtain a large tow carbon fiber after sizing;

[0088] Winding and collecting: Under a tension of 2720-2850 cN, a carbon fiber winder is used to wind and collect the sized large-tow carbon fiber to obtain the sized large-tow carbon fiber for reinforcing the rubber composite material.

[0089] Among them, the type of the pre-sizing agent is shown in Table 1, the properties of the pre-sizing agent, the molar ratio of resorcinol to formaldehyde in the secondary sizing agent RFL emulsion, the pre-sizing amount and the secondary sizing amount are shown in Table 2, and the pre-sizing drying and secondary sizing drying process parameters are shown in Table 3.

[0090] Among them, the brands of polyether polyurethane are: Crysol 6135, Crysol 6528, Crysol 6122, Crysol6140, Crysol 6126, and Crysol 6130.

[0091] Comparative Example 1

[0092] Comparative Example 1 is a method for manufacturing 120K carbon fiber, which is based on the method of Example 1, except that the sizing and drying process is as follows: unsized large-tow carbon fiber is sizing with a commercially available KTM-2S epoxy emulsion sizing agent, and horizontal hot air drying is performed at a drying temperature of 100°C.

[0093] Comparative Example 2

[0094] Comparative Example 2 is a method for manufacturing 120K carbon fiber, which is manufactured according to the method of Example 1, except that the RFL emulsion in Example 2 is used to size the unsized large tow carbon fiber, and the carbon fiber is dried horizontally using hot air at a drying temperature of 150°C.

[0095] Comparative Example 3

[0096] Comparative Example 3 is a method for manufacturing 120K carbon fiber, which is based on the method of Example 1, except that polyvinyl alcohol (PVA) water-based sizing agent is used to pre-size the unsized large-tow carbon fiber, and horizontal hot air drying is performed at a temperature of 80°C; then the RFL emulsion in Example 2 is used for secondary sizing at a drying temperature of 165°C.

[0097] Table 1 Table 2

[0098]

[0099]

[0100] Table 3

[0101]

[0102] ps: The "distance" in the table refers to the height between the carbon medium wave infrared radiator of the infrared radiation heating dryer and the carbon fiber

[0103] Test Case

[0104] The sized large tow carbon fibers prepared in the examples and comparative examples were tested for wear resistance and adhesion, and the results are shown in Table 4.

[0105] Table 4

[0106] Wear resistance (times) Adhesion force(N) Comparative Example 1 15600 105 Comparative Example 2 18300 113 Comparative Example 3 20650 122 Example 1 28700 155 Example 2 28260 158 Example 3 33100 151 Example 4 29540 148 Example 5 29830 165 Example 6 26920 150

[0107] From the results in the table, it can be seen that in Comparative Example 1, only the traditional epoxy emulsion is used, and in Comparative Example 2, only the RFL emulsion is used, the bonding force between the prepared carbon fiber and the rubber matrix is ​​low, and the wear resistance is poor. In Comparative Example 3, the contact angle and surface tension of the pre-sizing polyvinyl alcohol solution are too large, and the improvement effect is not obvious.

[0108] Examples 1-6 use a pre-sizing agent and RFL emulsion containing polyvinyl alcohol to which polyether polyurethane is added and with a contact angle of ≤35° and a surface tension of ≤80mN / m. Through a special sizing and drying process, the bonding strength between the carbon fiber and the rubber matrix is ​​significantly increased, the wear resistance is improved, and the overall improvement effect is obvious.

[0109] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized large tow carbon fiber, characterized in that: The method comprises: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding the polyacrylonitrile-based precursor to obtain the sizing large-tow carbon fiber; The sizing and drying comprises the following steps: Step 1: pre-sizing and pre-drying the washed carbon fiber tow using a pre-sizing agent containing polyvinyl alcohol and polyether polyurethane to obtain initial carbon fiber; Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber; Wherein, the contact angle of the pre-sizing agent is ≤35° and the surface tension is ≤80mN / m; The pre-drying method is heat-conducting oil hot roller drying; The secondary drying step comprises: performing infrared radiation drying and horizontal hot air drying in sequence.

2. The preparation method according to claim 1, wherein The contact angle of the pre-sizing agent is ≤10° and the surface tension is ≤75 mN / m.

3. The preparation method according to claim 1 or 2, wherein In the pre-sizing agent, the mass ratio of the polyvinyl alcohol to the polyether polyurethane is 1:0.6-0.9, preferably 1:0.7-0.

8.

4. The preparation method according to claim 1 or 2, wherein: The alcoholysis degree of the polyvinyl alcohol is 78-99%, preferably 88-92%; Preferably, the number average molecular weight of the polyvinyl alcohol is 20000-200000 g / mol, preferably 50000-150000 g / mol; Preferably, the number average molecular weight of the polyether polyurethane is 800-10000 g / mol, preferably 2000-6000 g / mol.

5. The preparation method according to claim 1 or 2, wherein: The polyether polyurethane comprises a structural unit A provided by a polyisocyanate and a structural unit B provided by a polyether polyol; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1; Preferably, the polyisocyanate is an aromatic polyisocyanate.

6. The preparation method according to claim 1 or 2, wherein: In step 1, the pre-drying temperature is 60-100°C, preferably 70-90°C.

7. The preparation method according to claim 1 or 2, wherein: In step 2, the temperature of the infrared radiation drying is 65-215°C, preferably 85-165°C; Preferably, the temperature of the horizontal hot air drying is 90-240°C, preferably 110-190°C.

8. The preparation method according to claim 1 or 2, wherein: In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:3-25, preferably 1:8-18.

9. The sized large-tow carbon fiber prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the sized large-tow carbon fiber according to claim 9 in reinforcing rubber composite materials.