Sizing large-tow carbon fiber for rubber-based composite material and preparation method of sizing large-tow carbon fiber

By employing a stepwise sizing and drying process, and using a combination of a specific pre-sizing agent and latex, the problem of poor bonding between sized large-tow carbon fibers and the rubber matrix was solved, achieving the preparation of carbon fibers with high impact resistance and strong adhesion, which is suitable for rubber-based composite materials.

CN118932718APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310536590.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of sized large-tow carbon fiber is complicated, and when used in rubber-based composite materials, it has poor impact resistance and weak adhesion to the rubber matrix.

Method used

By employing a stepwise sizing and drying process, a pre-sizing agent containing polyvinyl alcohol and aliphatic polyamide is used in combination with resorcinol formaldehyde latex. The pre-sizing agent with a contact angle ≤55° and a surface tension ≤40mN/m is prepared through infrared radiation drying and electrically heated roller drying, which significantly improves the adhesion and impact resistance of carbon fiber to the rubber matrix.

Benefits of technology

It enables simple and environmentally friendly industrial production, significantly improves the impact resistance and adhesion of sized large-tow carbon fiber-rubber composite materials, and has a post-impact compressive strength of over 440 MPa, making it suitable for existing carbon fiber industrial production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226498650000111
    Figure BDA0004226498650000111
  • Figure BDA0004226498650000112
    Figure BDA0004226498650000112
  • Figure BDA0004226498650000121
    Figure BDA0004226498650000121
Patent Text Reader

Abstract

The invention relates to the technical field of sizing large-tow carbon fiber preparation, in particular to sizing large-tow carbon fiber for a rubber-based composite material and a preparation method of the sizing large-tow carbon fiber. Comprising the following steps: carrying out pre-oxidation, low-temperature carbonization, high-temperature carbonization, surface treatment, water washing, sizing and drying, and winding to obtain sized large-tow carbon fiber, wherein polyacrylonitrile-based precursor is subjected to pre-oxidation, low-temperature carbonization, high-temperature carbonization, surface treatment, water washing, sizing and drying; the step of sizing and drying comprises the following steps: pre-sizing and pre-drying the washed carbon fibers by adopting a pre-sizing agent containing polyvinyl alcohol and aliphatic polyamide, and then carrying out secondary sizing and secondary drying on the initial carbon fibers by adopting resorcinol formaldehyde latex to obtain sized large-tow carbon fibers, the contact angle of the pre-sizing agent is less than or equal to 55 degrees and the surface tension is less than or equal to 40mN / m. The pre-drying is infrared radiation drying, and the secondary drying is electric heating hot roller drying and vertical hot air drying in sequence. The impact resistance of the sizing large-tow carbon fiber-rubber-based composite material is improved, and meanwhile, the bonding force of the sizing large-tow carbon fibers and a rubber matrix is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sizing large-tow carbon fiber preparation, and in particular to a sizing large-tow carbon fiber for rubber-based composite materials and a preparation method thereof. Background Art

[0002] Carbon fiber is one of the most widely used high-performance reinforcing materials. Composite materials made of carbon fiber as reinforcing phase and rubber as matrix are widely used in transportation equipment, industrial parts, sporting goods, energy and chemical industries. However, the surface and interfacial properties of carbon fiber and rubber matrix are very different, and it is difficult to effectively combine them into a solid integrated material, resulting in poor load transfer and failure to effectively play the reinforcing role of the fiber. Usually, a layer of epoxy sizing agent is coated on the surface of carbon fiber, but it cannot enhance the two-phase interaction with the rubber matrix. At the same time, carbon fiber is a brittle material with low elongation, and it is usually necessary to use a surface sizing agent to toughen and modify the fiber. High-performance sizing agents that can improve both fiber toughness and rubber interface performance are urgently needed to be developed.

[0003] CN104974471A discloses a method for preparing a high-heat-resistant and high-toughness epoxy resin carbon fiber composite material. Based on the core-shell rubber in the production process and combined with the excellent heat resistance of epoxy resin, the composite material has good high temperature resistance, high toughness and other characteristics during use. However, it is mainly based on the epoxy matrix and is not suitable for the preparation of rubber-based composite materials.

[0004] CN107459682A discloses a method for preparing a carbon fiber reinforced rubber composite material, wherein the carbon fiber is acidified, the roughness of the carbon fiber surface is increased, and the interfacial bonding between the fiber and the rubber matrix is ​​improved. However, the acidification treatment requires the consumption of a large amount of concentrated acid, which takes a long time and can only be performed intermittently, and is not suitable for a carbon fiber industrial production line. Moreover, the above schemes are unable to achieve good sizing of carbon fibers of 360K and above, thereby causing the large tow carbon fibers after sizing to have poor bonding strength with the rubber matrix when applied to rubber materials. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of the prior art that the preparation process of sized large tow carbon fiber is complicated, and when the prepared sized large tow carbon fiber is used in rubber-based composite materials, the impact resistance is poor and the bonding force between the sized large tow carbon fiber and the rubber matrix is ​​poor, and to provide a sized large tow carbon fiber for rubber-based composite materials and a preparation method thereof. On the one hand, the method is simple, continuous and low-cost to operate, and the preparation process is environmentally friendly and pollution-free, and is suitable for large-scale industrial production; on the other hand, the method can significantly improve the impact resistance of the sized large tow carbon fiber-rubber-based composite material prepared by the sized large tow carbon fiber while improving the bonding force between the prepared sized large tow carbon fiber and the rubber matrix through the process of step-by-step sizing and step-by-step drying, combined with a specific pre-sizing agent.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing sized large-tow carbon fibers for rubber-based composite materials, characterized in that the method comprises: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding the polyacrylonitrile-based precursor to obtain the sized large-tow carbon fibers;

[0007] The sizing and drying comprises the following steps:

[0008] Step 1: using a pre-sizing agent containing polyvinyl alcohol and aliphatic polyamide to pre-sizing and pre-dry the washed carbon fiber to obtain initial carbon fiber;

[0009] Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber;

[0010] Wherein, the contact angle of the pre-sizing agent is ≤55° and the surface tension is ≤40mN / m;

[0011] The pre-drying method is infrared radiation drying;

[0012] The secondary drying step includes: electrically heated hot roller drying and vertical hot air drying in sequence.

[0013] The second aspect of the present invention provides sized large-tow carbon fiber prepared by the preparation method described in the first aspect of the present invention.

[0014] Through the above technical scheme, the sized large tow carbon fiber for rubber-based composite materials and the preparation method thereof provided by the present invention achieve the following beneficial effects:

[0015] (1) The present invention can significantly improve the impact resistance of the sized large-tow carbon fiber-rubber-based composite material by introducing aliphatic polyamide into the pre-sizing agent, and the post-impact compressive strength is higher than 440 MPa, and the bonding force between the sized large-tow carbon fiber and the rubber matrix is ​​improved, which can reach 129N or above.

[0016] (2) The present invention selects a specific pre-sizing agent, controls the contact angle of the pre-sizing agent to be ≤55° and the surface tension to be ≤55 mN / m, and uses it in combination with resorcinol formaldehyde latex (hereinafter referred to as RFL emulsion), and combines the process of "pre-sizing-pre-drying-secondary sizing-secondary drying", wherein the pre-drying is infrared radiation drying, and the secondary drying is electric heating hot roller and vertical hot air drying in sequence, so as to improve the bonding force between the sized large-tow carbon fiber and the rubber matrix, and further improve the impact resistance of the sized large-tow carbon fiber-rubber-based composite material.

[0017] (3) The method of the present invention is applicable to the existing carbon fiber industrial production line, does not require much modification and upgrading, and has strong process adaptability; the sizing agent components and RFL emulsion used are low-cost and have broad industrial application prospects. DETAILED DESCRIPTION

[0018] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0019] The first aspect of the present invention provides a method for preparing sized large-tow carbon fibers for rubber-based composite materials, the method comprising: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding polyacrylonitrile-based precursor fibers to obtain the sized large-tow carbon fibers;

[0020] The sizing and drying comprises the following steps:

[0021] Step 1: using a pre-sizing agent containing polyvinyl alcohol and aliphatic polyamide to pre-sizing and pre-dry the washed carbon fiber to obtain initial carbon fiber;

[0022] Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber;

[0023] Wherein, the contact angle of the pre-sizing agent is ≤55° and the surface tension is ≤40mN / m;

[0024] The pre-drying method is infrared radiation drying;

[0025] The secondary drying step includes: electrically heated hot roller drying and vertical hot air drying in sequence.

[0026] In the present invention, the inventors have found that in the prior art, electrochemical treatment, acid-base treatment, surface sizing and other methods are generally used to improve the bonding problem between sized large-tow carbon fibers and rubber matrix. Among them, the most commonly used method is to use RFL emulsion to size the carbon fibers. However, due to the weak bonding ability of the RFL emulsion with the surface of the carbon fibers, the use of RFL emulsion alone cannot effectively improve the adhesion between the sized carbon fibers and the rubber matrix, nor can it simultaneously improve the impact resistance of the sized large-tow carbon fibers-rubber-based composite materials. After further research by the inventors, it was found that in the process of sizing the carbon fibers, a layer of hydrophilic pre-sizing agent is first coated on the surface of the carbon fibers, and then RFL emulsion is coated after drying, which can improve the bonding ability between the sized large-tow carbon fibers and the rubber matrix. However, any selection of a hydrophilic pre-sizing agent cannot achieve a good coupling effect with the RFL emulsion. For the pre-sizing agent described in the present invention, only when its contact angle is ≤55° and the surface tension is ≤40mN / m, can it achieve a good match with the RFL emulsion, and when the sized large-tow carbon fiber is applied to the rubber material, the bonding force between the sized large-tow carbon fiber and the rubber matrix is ​​improved. At the same time, the introduction of aliphatic polyamide into the pre-sizing agent can significantly improve the impact resistance of the sized large-tow carbon fiber-rubber-based composite material while ensuring the bonding force between the sized large-tow carbon fiber and the rubber matrix.

[0027] In the present invention, the pre-oxidation is carried out in an oxidation furnace with four heating temperature zones, the temperatures of the four heating temperature zones are respectively set to 0-250°C, 0-300°C, 0-300°C and 0-350°C, the total pre-oxidation time is 30-80min, the pre-oxidation time of each temperature zone is ensured to be the same, and the drawing ratios in the oxidation furnace of the four heating temperature zones are respectively 0-1.8, 0.8-1, 0.8-1 and 0.8-1.

[0028] In the present invention, the temperatures of the four heating zones, the total time of pre-oxidation and the drawing ratio are controlled to meet the above ranges, thereby achieving efficient and rapid pre-oxidation.

[0029] In the present invention, the low-temperature carbonization is carried out in an oxidation furnace with five heating temperature zones, and the temperatures of the five heating temperature zones are respectively set to 0-700°C, 0-700°C, 0-800°C, 0-950°C and 0-950°C. When the pre-oxidized carbon fiber is run in the low-temperature carbonization furnace, the draft ratio is controlled to be 1-1.2, and the total residence time in the low-temperature carbonization furnace is 1-10 minutes to obtain low-temperature carbonized fibers.

[0030] In the present invention, the high temperature carbonization process is carried out in an oxidation furnace with five heating temperature zones, wherein the temperatures of the five heating temperature zones are respectively 0-1300° C., 0-1400° C., 0-1700° C., 0-1900° C. and 0-2200° C. When the tow runs in the high temperature carbonization furnace, the draft ratio is controlled to be 0.6-0.95, and the total residence time in the high temperature carbonization furnace is 1-10 minutes to obtain high temperature carbonized filaments.

[0031] In the present invention, the surface treatment conditions include: using ammonium bicarbonate aqueous solution as electrolyte, voltage of 15-25V, electrolyte concentration of 20-30wt%, and treatment time of 50-80 seconds.

[0032] In the present invention, the water washing conditions include: washing at 50-60°C and a water flow rate of 5000-6500 L / h.

[0033] In the present invention, the winding and collecting can be carried out under a tension of 3000-3500 cN.

[0034] In the present invention, the term "large tow" refers to a large tow carbon fiber with more than 48,000 carbon fibers per bundle (abbreviated as 48K). According to a specific embodiment of the present invention, the large tow carbon fiber described in the present invention is 360K, that is, the number of carbon fibers per bundle is 360,000.

[0035] In the present invention, the preparation method of the pre-sizing agent can adopt the preparation method of the common emulsion in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0036] In the present invention, the surface tension refers to the surface tension when the material is diluted with water to a concentration of 2 wt %.

[0037] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber emulsion is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0038] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0039] According to the present invention, the contact angle of the pre-sizing agent is ≤10° and the surface tension is ≤35 mN / m.

[0040] According to the present invention, the average particle size of the aliphatic polyamide is ≤0.8 micrometer.

[0041] In the present invention, the average particle size of the aliphatic polyamide meets the above range, which can ensure that the pre-sizing agent is infiltrated and spread on the surface of the carbon fiber and improve its two-phase coupling effect.

[0042] Furthermore, the average particle size of the aliphatic polyamide is ≤0.5 micrometer.

[0043] According to the present invention, the mass ratio of the polyvinyl alcohol to the aliphatic polyamide is 1:0.3-1.

[0044] In the present invention, when the mass ratio of the polyvinyl alcohol to the aliphatic polyamide satisfies the above range, the impact resistance of the sized large tow carbon fiber-rubber composite material can be significantly improved while effectively improving the bonding force between the sized large tow carbon fiber and the rubber matrix.

[0045] Furthermore, the mass ratio of the polyvinyl alcohol to the aliphatic polyamide is 1:0.4-0.6.

[0046] In the present invention, the polyvinyl alcohol can be polyvinyl alcohol with different alcoholysis degrees, preferably partially alcoholysed polyvinyl alcohol.

[0047] According to the present invention, the alcoholysis degree of the polyvinyl alcohol is 78-99%, preferably 88-92%.

[0048] According to the present invention, the number average molecular weight of the polyvinyl alcohol is 20,000-200,000 g / mol, preferably 50,000-150,000 g / mol.

[0049] According to the present invention, the number average molecular weight of the aliphatic polyamide is 8000-45000 g / mol, preferably 15000-30000 g / mol.

[0050] According to one embodiment of the present invention, the aliphatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aliphatic dibasic acid.

[0051] In the present invention, “the aliphatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aliphatic dibasic acid” means that the aliphatic polyamide is prepared by polycondensation of a diamine and a dibasic acid.

[0052] In the present invention, when the aliphatic polyamide is added to the pre-sizing agent, compared with the aromatic polyamide, it is used in combination with the RFL emulsion to further improve the impact resistance of the sized large tow carbon fiber-rubber composite material prepared from the sized large tow carbon fiber and improve the bonding force between the sized carbon fiber and the rubber matrix.

[0053] In the present invention, the diamine can be commercially available, for example, it can be at least one of ethylenediamine, m-phenylenediamine, p-phenylenediamine, hexamethylenediamine, and decanediamine.

[0054] In the present invention, the aliphatic dibasic acid can be commercially available, for example, it can be at least one of oxalic acid, adipic acid, sebacic acid, and dodecanoic acid.

[0055] According to the present invention, the molar ratio of the structural unit A to the structural unit B is 1-2:1.

[0056] According to one embodiment of the present invention, the aliphatic polyamide comprises a structural unit C provided by a lactam.

[0057] In the present invention, “the aliphatic polyamide comprises a structural unit C provided by lactam” means that the aliphatic polyamide is prepared by ring-opening of lactam.

[0058] In the present invention, the lactam can be commercially available, for example, it can be at least one of valerolactam, caprolactam, β-lactam, and γ-lactam.

[0059] In the present invention, the aliphatic polyamide can be commercially available, for example, it can be SZ20, SZ50, SZ70, etc.

[0060] In the present invention, in order to further obtain sized large-tow carbon fibers with better comprehensive performance, aliphatic polyamide is preferably prepared by polycondensation of diamine and aliphatic dibasic acid.

[0061] According to the present invention, the pre-drying temperature is 60-100°C, preferably 70-90°C.

[0062] According to the present invention, the drying temperature of the electrically heated hot roller is 80-230°C, preferably 100-180°C.

[0063] According to the present invention, the temperature of the vertical hot air drying is 90-240°C, preferably 110-190°C.

[0064] In the present invention, the infrared radiation drying can be performed using an infrared radiation drying machine, and the infrared radiation heating drying machine contains a carbon medium-wave infrared radiator.

[0065] In the present invention, when infrared radiation drying is performed, the distance between the carbon medium wave infrared radiator of the infrared radiation heating dryer and the carbon fiber is 40-80 mm, and the power density is 20-50 kW / m 2 .

[0066] According to the present invention, in the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:3-25, preferably 1:8-18.

[0067] According to the present invention, based on the mass of the washed carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%;

[0068] According to the present invention, based on the mass of the washed carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

[0069] In the present invention, the prepared sized large-tow carbon fiber can be used in a reinforced rubber composite material, wherein the content of the sized large-tow carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0070] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0071] In the present invention, there is no particular limitation on the type of the rubber material, and it may be, for example, acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, butyl rubber, etc., preferably the same type as the rubber emulsion in the RFL emulsion.

[0072] The second aspect of the present invention provides sized large-tow carbon fiber prepared by the preparation method described in the first aspect of the present invention.

[0073] The present invention will be described in detail below by way of examples. In the following examples, each parameter is obtained by the following method.

[0074] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0075] Surface tension: The pre-sizing agent was diluted to a concentration of 2 wt % and the surface tension was tested using a dynamic surface tension meter at a temperature of 25°C.

[0076] Adhesion: The sized large tow carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sized large tow carbon fiber is 20% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sized large tow carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out 1 cm of length is the adhesion between the fiber and the rubber.

[0077] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0078] Compression strength after impact: Referring to SACMA SRM 2R-94 standard, a 6.7 J / mm drop hammer impact is applied to the center of the sized large-tow carbon fiber-rubber composite sample to calculate the compression strength after impact.

[0079] KTM-4 epoxy emulsion, purchased from Sinopharm Reagent;

[0080] Polyvinyl alcohol (PVA) was purchased from Sinopharm.

[0081] Aliphatic polyamides SZ20, SZ50, and SZ70 were purchased from Sinopharm Reagents.

[0082] Examples 1-6

[0083] Embodiments 1-6 are methods for producing uniform 360K carbon fibers, comprising:

[0084] Pre-oxidation: The polyacrylonitrile-based precursor passes through oxidation furnace No. 1, oxidation furnace No. 2, oxidation furnace No. 3, and oxidation furnace No. 4 for pre-oxidation treatment. The temperatures of the four heating temperature zones are 239°C, 250°C, 261°C, and 272°C, respectively. The pre-oxidation time in each temperature zone is the same, and the total pre-oxidation time is 44 minutes. The draft ratios between the oxidation furnaces in the four heating temperature zones are 1.27, 0.96, 0.96, and 0.95, respectively;

[0085] Low-temperature carbonization: Using nitrogen as the medium, the pre-oxidized filament bundles are sequentially passed through a low-temperature carbonization furnace with five heating temperature zones at 540°C, 650°C, 710°C, 820°C, and 885°C, respectively. The draft ratio of each zone is controlled to be 1.1, and the total residence time in the low-temperature carbonization furnace is 1.2 minutes to obtain low-temperature carbonized filaments.

[0086] High temperature carbonization: With nitrogen as the medium, the filament bundle passes through a high temperature carbonization furnace with five heating temperature zones at 958°C, 1270°C, 1310°C, 1380°C and 1460°C respectively, and the draft ratio of each zone is controlled to be 0.83. The total residence time in the high temperature carbonization furnace is 1.2 minutes to obtain high temperature carbonized filaments;

[0087] Surface treatment: The high-temperature carbonized fibers are passed through a traction device into a surface treatment tank, with an ammonium bicarbonate aqueous solution as the electrolyte, a voltage of 22V, an electrolyte concentration of 25wt%, and a treatment time of 60 seconds to obtain surface-treated carbon fibers;

[0088] Water washing: washing the surface-treated carbon fiber at a water flow rate of 5800 L / h and a water washing temperature of 56° C. to obtain a washed carbon fiber tow;

[0089] Sizing and drying: The washed carbon fiber tow is directly introduced into the first sizing tank for pre-sizing, and then passed through the infrared radiation dryer for pre-drying under the set process parameters; then enters the second sizing tank for secondary sizing, and then passes through the electric heating hot roller and the vertical hot air dryer in turn for secondary drying under the set process parameters to obtain the sized large tow carbon fiber;

[0090] Winding and collecting: Under a tension of 3060-3270 cN, a carbon fiber winder is used to wind and collect the sizing large-tow carbon fiber to obtain the sizing large-tow carbon fiber.

[0091] Among them, the type of the pre-sizing agent is shown in Table 1, the properties of the pre-sizing agent, the molar ratio of resorcinol to formaldehyde in the secondary sizing agent RFL emulsion, the pre-sizing amount and the secondary sizing amount are shown in Table 2, and the pre-sizing drying and secondary sizing drying process parameters are shown in Table 3.

[0092] Comparative Example 1

[0093] Comparative Example 1 is a method for manufacturing 360K carbon fiber, which is manufactured according to the method of Example 1, except that the sizing and drying process is as follows: sizing the unsized large tow carbon fiber with a commercially available KTM-4 epoxy emulsion sizing agent, vertical hot air drying, and a drying temperature of 100° C. Winding and collecting the filaments to prepare the sized large tow carbon fiber.

[0094] Comparative Example 2

[0095] Comparative Example 2 is a method for manufacturing 360K carbon fiber, which is prepared according to the method of Example 1, except that the RFL emulsion in Example 2 is used to size the unsized large-tow carbon fiber, and the fiber is dried vertically at a temperature of 150°C, and the sized large-tow carbon fiber is prepared by winding and collecting the fiber.

[0096] Comparative Example 3

[0097] Comparative Example 3 is a method for manufacturing 360K carbon fiber, which is manufactured according to the method of Example 1, except that the unsized large-tow carbon fiber is sized with the RFL emulsion in Example 2, and vertical hot air drying is performed at a temperature of 80°C. The carbon fiber is then sized for a second time with the RFL emulsion in Example 2, and the drying temperature is 165°C. The sized large-tow carbon fiber is prepared by winding and collecting the yarn.

[0098] Table 1

[0099]

[0100] Table 2

[0101]

[0102] Table 3

[0103] ps: The "distance" in the table refers to the height between the carbon medium wave infrared radiator of the infrared radiation heating dryer and the carbon fiber

[0104] Test Case

[0105] The sized large tow carbon fiber prepared in the embodiment and the comparative example and the rubber matrix were prepared into a sized large tow carbon fiber-rubber matrix composite material, and the adhesion test was carried out. The post-impact compression strength of the sized large tow carbon fiber-rubber composite material was tested with reference to the SACMA SRM 2R-94 standard. The results are shown in Table 4.

[0106] Table 4

[0107]

[0108]

[0109] As can be seen from the results in the table, in Comparative Example 1, only the traditional epoxy emulsion is used as the sizing agent, and in Comparative Example 2, only the RFL emulsion is used as the sizing agent. The prepared sized large tow carbon fibers have low bonding strength with the rubber matrix and low impact resistance. The pre-sizing agent used in Comparative Example 3 contains only polyvinyl alcohol, and the surface tension is too large, so the improvement effect is not good.

[0110] Examples 1-6 use a pre-sizing agent containing polyvinyl alcohol to which aliphatic polyamide is added and has a contact angle of ≤55° and a surface tension of ≤40mN / m, and are used in combination with an RFL emulsion. Through a special sizing and drying process, the carbon fibers finally prepared have good adhesion to the rubber matrix and excellent impact resistance, with a post-impact compressive strength of not less than 400MPa.

[0111] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized large-tow carbon fibers for rubber-based composite materials, It is characterized in that The method comprises: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding the polyacrylonitrile-based precursor to obtain the sizing large-tow carbon fiber; The sizing and drying comprises the following steps: Step 1: using a pre-sizing agent containing polyvinyl alcohol and aliphatic polyamide to pre-sizing and pre-dry the washed carbon fiber to obtain initial carbon fiber; Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber; Wherein, the contact angle of the pre-sizing agent is ≤55° and the surface tension is ≤40mN / m; The pre-drying method is infrared radiation drying; The secondary drying step includes: electrically heated hot roller drying and vertical hot air drying in sequence.

2. The preparation method according to claim 1, in, The contact angle of the pre-sizing agent is ≤10° and the surface tension is ≤35mN / m; Preferably, the average particle size of the aliphatic polyamide is ≤0.8 micrometer, preferably ≤0.5 micrometer.

3. The method according to claim 1 or 2, in, The mass ratio of the polyvinyl alcohol to the aliphatic polyamide is 1:0.3-0.8, preferably 1:0.4-0.

6.

4. The method according to claim 1 or 2, in, The alcoholysis degree of the polyvinyl alcohol is 78-99%, preferably 88-92%; Preferably, the number average molecular weight of the polyvinyl alcohol is 20000-200000 g / mol, preferably 50000-150000 g / mol; Preferably, the number average molecular weight of the aliphatic polyamide is 8000-45000 g / mol, preferably 15000-30000 g / mol.

5. The method according to claim 1 or 2, in, The aliphatic polyamide comprises a structural unit A provided by a diamine and a structural unit B provided by an aliphatic dibasic acid; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1; Alternatively, the aliphatic polyamide comprises structural units C provided by lactam.

6. The method according to claim 1 or 2, in, In step 1, the pre-drying temperature is 60-100°C, preferably 70-90°C.

7. The method according to claim 1 or 2, in, In step 2, the temperature of the electrically heated hot roller drying is 80-230°C, preferably 100-180°C; Preferably, the vertical hot air drying temperature is 90-240°C, preferably 110-190°C.

8. The preparation method according to claim 1 or 2, in, In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:3-25, preferably 1:8-18.

9. The preparation method according to claim 1 or 2, in, Based on the weight of the washed carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%; Preferably, based on the mass of the washed carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

10. The sized large-tow carbon fiber prepared by the preparation method according to any one of claims 1 to 9.