Device and method for producing cement through flame-proof combustion of low-carbon-emission limestone
By adopting low-carbon emission limestone flame-free combustion device and oxygen-rich combustion technology in cement production, the problems of heat loss and environmental pollution in traditional cement production are solved, and efficient and environmentally friendly carbon dioxide collection and pure cement clinker production are achieved, improving the production of high-quality carbon dioxide The strength and construction performance of concrete are achieved.
Patent Information
- Application Number
- CN202411235433.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
In traditional cement production, heat loss and environmental pollution caused by air combustion, high carbon emissions, low activity of fly ash affects the strength and durability of concrete, and the construction performance is unstable.
Using a low-carbon emission limestone flame-separating combustion device, the preheating section, calcining section and cooling section of the calciner is combined with an oxygen-rich combustion chamber to generate high concentrations of carbon dioxide and remove dust, avoid the formation of nitrogen oxides, and use the richness of pulverized coal and oxygen. Oxygen combustion generates heat for calcining limestone, producing high concentrations of carbon dioxide and pure cement clinker.
It reduces fuel consumption and cost, reduces carbon emissions, produces high purity and good environmental protection performance, avoids nitrogen oxide pollution, and improves the strength and construction performance of concrete.
Smart Images

Figure CN118936020A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement industry, and more particularly to a device and method for producing cement by low-carbon emission limestone muffle combustion. Background Art
[0002] Traditional cement production uses air as a combustion aid. 21% of the oxygen in the air participates in combustion, while 78% of the nitrogen does not participate in combustion. A large amount of nitrogen is heated unnecessarily and discharged into the atmosphere at high temperatures, causing a large amount of heat loss and high fuel consumption. At the same time, nitrogen reacts with oxygen at high temperatures to produce NO x , NO x The gas is easily discharged into the atmosphere to form acid rain and cause environmental pollution. The cement industry is the second largest CO2 emission industry in my country, second only to the thermal power industry in terms of carbon emissions. The concentration of carbon dioxide in the flue gas produced by calcining limestone in an air atmosphere is diluted by nitrogen. The cost of capturing and concentrating the carbon dioxide in this diluted flue gas is relatively high. In the conventional calcination process, the fuel combustion process and the limestone decomposition process are completed in the same kiln. The gas in the kiln includes carbon dioxide, nitrogen, a small amount of oxygen, and a certain amount of dust. If the calcination fuel of limestone is solid fuel, such as coal powder, coal blocks, etc., the produced cement clinker will be mixed with some impurities, which will affect the quality of the product, mainly manifested in: (1) Impact on strength and durability: Fly ash has low silicate activity, which means that its contribution to concrete strength may not be as good as other materials; when the amount of fly ash added is too high, the strength of concrete may be affected and reduced; in addition, certain compounds in fly ash may increase the intrusion of chloride ions in concrete, thereby increasing the risk of steel corrosion and having an adverse effect on the durability of concrete. (2) Impact on gelation time and setting properties: Due to the low silicate activity of fly ash, its hydration reaction rate is relatively slow. (3) Impact on construction performance: The particle morphology and characteristics of fly ash may change the fluidity and workability of concrete; when the dosage is too high, the fluidity of concrete may be reduced, making construction more difficult. (4) Impact caused by the instability of fly ash quality: The properties and quality of fly ash are affected by many factors, such as coal combustion method, combustion temperature, coal type and coal quality; this instability may have an adverse effect on the overall performance and consistency of concrete. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide a device and method for producing cement by low-carbon emission limestone flame muffle combustion, which can produce high-concentration carbon dioxide, facilitate collection and resource utilization, reduce costs, and at the same time, the flue gas after combustion does not contain nitrogen compounds, will not cause environmental pollution, and has good environmental protection performance.
[0004] The present invention provides a device for producing cement by low-carbon emission limestone muffle combustion, comprising:
[0005] The calcining furnace body is composed of a preheating section, a calcining section and a cooling section from top to bottom; the top of the preheating section is provided with a limestone feed port and a flue gas outlet, and the side wall is provided with a carbon dioxide outlet; the middle of the calcining section is provided with an oxygen-enriched combustion chamber, and the side wall is provided with pulverized coal and oxygen inlets communicating with the oxygen-enriched combustion chamber; the bottom of the cooling section is provided with a cement discharge port and a coal slag outlet;
[0006] The top of the oxygen-enriched combustion chamber is communicated with the smoke outlet through a gas phase pipeline, and the bottom of the oxygen-enriched combustion chamber is communicated with the coal ash outlet through a solid phase pipeline.
[0007] Preferably, the inner wall of the calcining furnace is provided with a plurality of rectifying folding plates.
[0008] Preferably, the carbon dioxide outlet is connected to a dust removal device; the dust removal device is provided with a dust outlet and a gas phase outlet; the gas phase outlet is connected to a carbon dioxide collection unit.
[0009] The present invention also provides a method for producing cement by low-carbon emission limestone muffle combustion, using the device described in the above technical solution, comprising the following steps:
[0010] The crushed limestone particles are fed into the preheating section through the limestone feed port for preheating, and then fed into the calcining section for calcination to obtain cement clinker and carbon dioxide respectively; the cement clinker is cooled in the cooling section and then discharged from the cement discharge port; the carbon dioxide is discharged from the carbon dioxide outlet;
[0011] Pulverized coal and oxygen are introduced into the oxygen-enriched combustion chamber of the calcining section through the pulverized coal and oxygen inlet for oxygen-enriched combustion, generating heat for calcination in the calcining section to obtain flue gas, ash and coal slag respectively; the flue gas is mixed with the carbon dioxide generated by the calcination of limestone through the flue gas outlet, and high-concentration carbon dioxide is obtained after dust removal; the ash and coal slag are discharged from the coal slag outlet.
[0012] Preferably, the particle size of the crushed limestone particles is 7.5 mm to 15.0 mm, and the processing capacity is 5000 t / d to 6000 t / d.
[0013] Preferably, the preheating temperature is 750° C. to 870° C., and the preheating time is 5 min to 8 min.
[0014] Preferably, the calcination temperature is 1370° C. to 1450° C., and the calcination time is 12 min to 15 min.
[0015] Preferably, the cooling temperature is 900° C. to 930° C., and the cooling time is 8 min to 10 min.
[0016] Preferably, the amount of pulverized coal is 200t / d~400t / d; and the oxygen-coal ratio is 2.05~2.15.
[0017] Preferably, after the carbon dioxide is discharged from the carbon dioxide outlet, it is dedusted by a dust removal device to obtain dust and carbon dioxide respectively; the dust is discharged from the dust outlet; the carbon dioxide enters the carbon dioxide collection unit;
[0018] The dust removal efficiency is greater than or equal to 99%, and the dust concentration in the carbon dioxide after dust removal is less than 50mg / Nm 3 .
[0019] The present invention provides a device and method for producing cement by low-carbon emission limestone flame-muffle combustion; the device comprises: a calcining furnace body; the calcining furnace body is composed of a preheating section, a calcining section and a cooling section from top to bottom; the top of the preheating section is provided with a limestone feed port and a flue gas outlet, and the side wall is provided with a carbon dioxide outlet; the middle of the calcining section is provided with an oxygen-enriched combustion chamber, and the side wall is provided with a pulverized coal and oxygen inlet connected to the oxygen-enriched combustion chamber; the bottom of the cooling section is provided with a cement discharge port and a slag outlet; the top of the oxygen-enriched combustion chamber is connected to the flue gas outlet through a gas phase pipeline, and the bottom is connected to the slag outlet through a solid phase pipeline. Compared with the prior art, the device provided by the present invention adopts a specific structure and connection relationship to achieve better overall interaction, can produce high-concentration carbon dioxide, which is conducive to collection and resource utilization, and at the same time, the flue gas after oxygen-enriched combustion does not contain nitrogen compounds, and the carbon dioxide concentration is high, which is convenient for collection and resource utilization. Compared with air combustion, oxygen-enriched combustion saves the heat required for heating nitrogen, has high thermal efficiency, saves fuel, and reduces costs.
[0020] In addition, the cement clinker produced by the present invention has high purity, is convenient for preparing and dispensing special cement, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of the structure of a device for producing cement by low-carbon emission limestone flame muffle combustion provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The present invention provides a device for producing cement by low-carbon emission limestone muffle combustion, comprising:
[0024] The calcining furnace body is composed of a preheating section, a calcining section and a cooling section from top to bottom; the top of the preheating section is provided with a limestone feed port and a flue gas outlet, and the side wall is provided with a carbon dioxide outlet; the middle of the calcining section is provided with an oxygen-enriched combustion chamber, and the side wall is provided with pulverized coal and oxygen inlets communicating with the oxygen-enriched combustion chamber; the bottom of the cooling section is provided with a cement discharge port and a coal slag outlet;
[0025] The top of the oxygen-enriched combustion chamber is communicated with the smoke outlet through a gas phase pipeline, and the bottom of the oxygen-enriched combustion chamber is communicated with the coal ash outlet through a solid phase pipeline.
[0026] See also Figure 1 , Figure 1 A schematic structural diagram of an apparatus for producing cement by low-carbon emission limestone flame muffle combustion provided in an embodiment of the present invention; wherein 1 is a calcining furnace body, 2 is a calcining section, 3 is a pulverized coal and oxygen inlet, 4 is a cooling section, 5 is a preheating section, 6 is a limestone feed port, 7 is a flue gas outlet, 8 is a carbon dioxide outlet, 9 is a dust removal device, 10 is a carbon dioxide collection unit, 11 is a dust outlet, 12 is a rectifying folding plate, 13 is a cement discharge port, 14 is a coal ash outlet, and 15 is an oxygen-enriched combustion chamber.
[0027] In the present invention, the device for producing cement by low-carbon emission limestone muffle combustion mainly comprises: a calcining furnace body (1), a calcining section (2), a pulverized coal and oxygen inlet (3), a cooling section (4), a preheating section (5), a limestone feed inlet (6), a flue gas outlet (7), a carbon dioxide outlet (8), a dust removal device (9), a carbon dioxide collection unit (10), a dust outlet (11), a rectifying folding plate (12), a cement discharge port (13), a coal ash outlet (14) and an oxygen-enriched combustion chamber (15); wherein the limestone feed inlet (6) is connected to the preheating section (5) of the calcining furnace body (1). The calcining section (2) is connected to the preheating section (5) and the cooling section (4) respectively; the preheating section (5) is connected to the carbon dioxide outlet (8); the carbon dioxide outlet (8) is connected to the inlet of the dust removal device (9); the dust removal device (9) is connected to the inlet of the carbon dioxide collection unit (10) and the dust outlet (11) respectively; the cooling section (4) is connected to the cement discharge port (13); the pulverized coal and oxygen inlet (3) is connected to the oxygen-enriched combustion chamber (15); the oxygen-enriched combustion chamber (15) is connected to the flue gas outlet (7) and the coal ash outlet (14) respectively; the flue gas outlet (7) is connected to the carbon dioxide outlet (8).
[0028] In the present invention, the calcining furnace body (1) is composed of a preheating section (5), a calcining section (2) and a cooling section (4) from top to bottom, forming an integral furnace body structure. In the present invention, the inner wall of the calcining furnace body is preferably provided with a plurality of rectifying folding plates.
[0029] In the present invention, the top of the preheating section (5) is provided with a limestone feed port (6) and a flue gas outlet (7), and the side wall is provided with a carbon dioxide outlet (8). In the present invention, the carbon dioxide outlet (8) is preferably connected to a dust removal device (9); the dust removal device is provided with a dust outlet (11) and a gas phase outlet; the gas phase outlet is connected to a carbon dioxide collection unit (10). In the present invention, the carbon dioxide collection unit (10) is preferably a carbon dioxide storage tank; the carbon dioxide storage tank is preferably provided with a pressure gauge, a thermometer and a safety valve.
[0030] In the present invention, an oxygen-enriched combustion chamber (15) is provided in the middle of the calcining section (2), and a pulverized coal and oxygen inlet (3) communicating with the oxygen-enriched combustion chamber (15) is provided on the side wall.
[0031] In the present invention, a cement discharge port (13) and a coal slag outlet (14) are provided at the bottom of the cooling section (4).
[0032] In the present invention, the top end of the oxygen-enriched combustion chamber (15) is connected to the flue gas outlet (7) via a gas phase pipeline, and the bottom end is connected to the coal ash outlet (14) via a solid phase pipeline.
[0033] In a preferred embodiment of the present invention, flow detection and control devices are provided on the connecting pipelines between the limestone feed port (6) and the pulverized coal and oxygen inlet (3) and the flue gas outlet (7), and all flow detection and control devices are connected to the control unit of the system; flow detection and control devices are provided on the connecting pipelines between the limestone feed port (6) and the cement discharge port (13), and all flow detection and control devices are connected to the control unit of the system; flow detection and control devices are provided on the connecting pipelines between the pulverized coal and oxygen inlet (3) and the coal ash outlet (14) and the flue gas outlet (7), and all flow detection and control devices are connected to the control unit of the system.
[0034] The present invention provides a flow detection and control device on the connecting pipeline between the pulverized coal and oxygen inlet (3) and the flue gas outlet (7), which can coordinately control the heat generated by the oxygen-enriched combustion of the pulverized coal, control the decomposition temperature of the limestone in the calcining section (2), and accurately control the temperature of the entire calcining section (2); a flow detection and control device is provided on the connecting pipeline between the limestone feed port (6) and the cement discharge port (13), and by detecting and controlling the limestone feed amount, the limestone feed amount and the cement clinker discharge amount can be coordinated, thereby controlling the calcination time of the entire calcining furnace; a flow detection and control device is provided on the connecting pipeline between the pulverized coal input amount and the oxygen input amount of the pulverized coal and oxygen inlet (3), which can coordinately control the oxygen-coal ratio entering the oxygen-enriched combustion of the pulverized coal, and control the composition of the pulverized coal combustion product.
[0035] On this basis, the pulverized coal generates a large amount of heat through oxygen-enriched combustion, which is used to calcine limestone, decomposing it into cement clinker and carbon dioxide. The ash produced after the oxygen-enriched combustion of the pulverized coal is discharged from the coal slag outlet. The limestone enters the calcining furnace through the feed port after being crushed, and enters the calcining section after being preheated to undergo calcination and decomposition reactions. The generated cement clinker flows out from the cement outlet. The above-mentioned low-carbon emission limestone flame-muffle combustion device for producing cement ensures that the oxygen-enriched combustion of the pulverized coal and the calcination of the limestone transfer heat but not mass. The generated flue gas and decomposition gas have a high carbon dioxide concentration, which is conducive to the collection of carbon dioxide and downstream resource utilization, reducing costs. The oxygen-enriched combustion isolates nitrogen, avoids the generation of nitrogen oxides, and has good environmental performance. At the same time, the generated cement clinker is not mixed with coal slag, which is convenient for the subsequent blending of special cement ratios.
[0036] The present invention also provides a method for producing cement by low-carbon emission limestone muffle combustion, using the device described in the above technical solution, comprising the following steps:
[0037] The crushed limestone particles are fed into the preheating section through the limestone feed port for preheating, and then fed into the calcining section for calcination to obtain cement clinker and carbon dioxide respectively; the cement clinker is cooled in the cooling section and then discharged from the cement discharge port; the carbon dioxide is discharged from the carbon dioxide outlet;
[0038] Pulverized coal and oxygen are introduced into the oxygen-enriched combustion chamber of the calcining section through the pulverized coal and oxygen inlet for oxygen-enriched combustion, generating heat for calcination in the calcining section to obtain flue gas, ash and coal slag respectively; the flue gas is mixed with the carbon dioxide generated by the calcination of limestone through the flue gas outlet, and high-concentration carbon dioxide is obtained after dust removal; the ash and coal slag are discharged from the coal slag outlet.
[0039] In the present invention, the particle size of the crushed limestone particles is preferably 7.5 mm to 15.0 mm, and the processing capacity is preferably 5000 t / d to 6000 t / d, more preferably 5500 t / d.
[0040] In the present invention, the preheating temperature is preferably 750°C to 870°C, more preferably 800°C to 820°C, and the flue gas generated by the oxygen-enriched combustion of pulverized coal preheats the limestone particles in the preheating section (5); the preheating time is preferably 5 min to 8 min.
[0041] In the present invention, the calcination temperature is preferably 1370° C. to 1450° C., more preferably 1400° C. to 1420° C., and the calcination time is preferably 12 min to 15 min.
[0042] In the present invention, the cooling temperature is preferably 900° C. to 930° C., more preferably 905° C. to 925° C., and the cooling time is preferably 8 min to 10 min.
[0043] In the present invention, the amount of pulverized coal is preferably 200 t / d to 400 t / d, more preferably 300 t / d to 320 t / d; the oxygen-coal ratio is preferably 2.05 to 2.15.
[0044] In the present invention, the carbon dioxide is discharged from the carbon dioxide outlet (8) and then removed by a dust removal device (9) to obtain dust and carbon dioxide respectively; the dust is discharged from the dust outlet (11); the carbon dioxide enters the carbon dioxide collection unit (10); the efficiency of the dust removal is preferably greater than or equal to 99%, and the dust concentration in the carbon dioxide after the dust removal is preferably less than 50 mg / Nm 3 .
[0045] The method for producing cement by low-carbon emission limestone flame-muffle combustion provided by the present invention adopts pulverized coal oxygen-enriched flame-muffle combustion to decompose limestone into cement clinker and carbon dioxide at high temperature. The generated carbon dioxide has a high concentration, which is convenient for capture and resource utilization. The produced cement clinker has high purity, which is convenient for the proportioning and blending of special cement. The flue gas generated by the pulverized coal oxygen-enriched combustion does not contain nitrogen oxides, and has a high carbon dioxide concentration, which is convenient for capture and resource utilization.
[0046] The present invention provides a device and method for producing cement by low-carbon emission limestone flame-muffle combustion; the device comprises: a calcining furnace body; the calcining furnace body is composed of a preheating section, a calcining section and a cooling section from top to bottom; a limestone feed port and a flue gas outlet are provided at the top of the preheating section, and a carbon dioxide outlet is provided on the side wall; an oxygen-enriched combustion chamber is provided in the middle of the calcining section, and a pulverized coal and oxygen inlet connected to the oxygen-enriched combustion chamber is provided on the side wall; a cement discharge port and a coal ash outlet are provided at the bottom of the cooling section; the top of the oxygen-enriched combustion chamber is connected to the flue gas outlet through a gas phase pipeline, and the bottom is connected to the coal ash outlet through a solid phase pipeline. Compared with the prior art, the device provided by the present invention adopts a specific structure and connection relationship to achieve better overall interaction, can produce high-concentration carbon dioxide, is conducive to collection and resource utilization, and reduces costs. At the same time, the flue gas after oxygen-enriched combustion does not contain nitrogen compounds, will not cause environmental pollution, and has good environmental protection performance.
[0047] In addition, the cement clinker produced by the present invention has high purity, is convenient for preparing and dispensing special cement, and has broad application prospects.
[0048] In order to further illustrate the present invention, the following examples are used to provide a detailed description. The limestone used in the following examples of the present invention is provided by Karamay Jiuhong Cement Co., Ltd.
[0049] Example
[0050] The present invention adopts the device for producing cement by low-carbon emission limestone muffle combustion as described in the above technical solution, see Figure 1As shown; wherein, 1 is the calcining furnace body, 2 is the calcining section, 3 is the pulverized coal and oxygen inlet, 4 is the cooling section, 5 is the preheating section, 6 is the limestone feed inlet, 7 is the flue gas outlet, 8 is the carbon dioxide outlet, 9 is the dust removal device, 10 is the carbon dioxide collection unit, 11 is the dust outlet, 12 is the rectifying folding plate, 13 is the cement discharge port, 14 is the coal ash outlet, and 15 is the oxygen-enriched combustion chamber.
[0051] The specific working process of the above-mentioned low-carbon emission limestone muffle combustion cement production device is as follows:
[0052] The crushed limestone particles (particle size of 7.5-15.0 mm, shape close to sphere or cube; processing scale of 5500 t / d) enter the preheating section (5) of the calcining furnace through the limestone feed port (6), and enter the calcining section (2) after being preheated at 810°C±10°C for 5min~8min. After being calcined at 1410°C±10°C for 12min~15min, they are decomposed into cement clinker and carbon dioxide. The cement clinker is discharged from the cement discharge port (13) after passing through the cooling section (4) (cooling temperature of 915°C±10°C, residence time of 8min~10min), and the carbon dioxide gas is discharged from the carbon dioxide outlet (8). After passing through the dust removal device (9) (dust removal efficiency of 99%, outlet dust concentration <50mg / Nm 3 ) to separate dust and carbon dioxide, wherein the dust is discharged from the dust outlet (11) and the carbon dioxide enters the carbon dioxide collection storage tank (10); pulverized coal and oxygen (coal feed rate is 311.52 t / d, oxygen-coal ratio is 2.12-2.15) enter the oxygen-enriched combustion chamber (15) of the calcining section (2) from the pulverized coal and oxygen inlet (3), and a large amount of heat generated by the oxygen-enriched combustion is used to calcine limestone. The flue gas generated by the oxygen-enriched combustion is mixed with the carbon dioxide generated by the calcination of limestone through the flue gas outlet (7), and high-concentration carbon dioxide is obtained after dust removal by the dust removal device (9). Ash and slag generated by the oxygen-enriched combustion of pulverized coal are discharged from the slag outlet (14).
[0053] The experimental results are shown in the following table:
[0054] Based on a limestone processing scale of 5,500 t / d, the total CO2 emissions in the system are reduced by approximately 1.0686 million tons / year compared with traditional limestone calcination processes and traditional coal-to-olefin processes.
[0055] Cement clinker 3CaO·Al2O3≤3.0, 3CaO·SiO2≤52.0, belongs to high-resistant clinker.
[0056] In summary, compared with the prior art, the present invention has the following beneficial technical effects:
[0057] The present invention provides a low-carbon emission limestone flame-muffle combustion cement production device and method. The pulverized coal generates a large amount of heat through oxygen-enriched combustion for calcining limestone, so that it is decomposed into cement clinker and carbon dioxide. The ash produced after the oxygen-enriched combustion of the pulverized coal is discharged from the furnace through the coal slag outlet. The limestone enters the calcining furnace through the feed port after being crushed, and enters the calcining section after being preheated to undergo calcination and decomposition reaction. The generated cement clinker flows out from the cement discharge port. The device and method can produce high-concentration carbon dioxide, which is conducive to collection and resource utilization, and reduces costs. The flue gas after oxygen-enriched combustion does not contain nitrogen compounds, and the carbon dioxide concentration is high, which is conducive to collection and resource utilization. At the same time, the produced cement clinker has high purity, which is convenient for the preparation and deployment of special cement.
[0058] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A device for producing cement by low-carbon emission limestone muffle combustion, include: The calcining furnace body is composed of a preheating section, a calcining section and a cooling section from top to bottom; the top of the preheating section is provided with a limestone feed port and a flue gas outlet, and the side wall is provided with a carbon dioxide outlet; the middle of the calcining section is provided with an oxygen-enriched combustion chamber, and the side wall is provided with pulverized coal and oxygen inlets communicating with the oxygen-enriched combustion chamber; the bottom of the cooling section is provided with a cement discharge port and a coal slag outlet; The top of the oxygen-enriched combustion chamber is communicated with the smoke outlet through a gas phase pipeline, and the bottom of the oxygen-enriched combustion chamber is communicated with the coal ash outlet through a solid phase pipeline.
2. The device for producing cement by low-carbon emission limestone muffle combustion according to claim 1, It is characterized in that The inner wall of the calcining furnace is provided with a plurality of rectifying folding plates.
3. The device for producing cement by low-carbon emission limestone muffle combustion according to claim 1, It is characterized in that The carbon dioxide outlet is connected to a dust removal device; the dust removal device is provided with a dust outlet and a gas phase outlet; the gas phase outlet is connected to a carbon dioxide collection unit.
4. A method for producing cement by low carbon emission limestone muffle combustion, It is characterized in that The device according to claim 1 comprises the following steps: The crushed limestone particles are fed into the preheating section through the limestone feed port for preheating, and then fed into the calcining section for calcination to obtain cement clinker and carbon dioxide respectively; the cement clinker is cooled in the cooling section and then discharged from the cement discharge port; the carbon dioxide is discharged from the carbon dioxide outlet; Pulverized coal and oxygen are introduced into the oxygen-enriched combustion chamber of the calcining section through the pulverized coal and oxygen inlet for oxygen-enriched combustion, generating heat for calcination in the calcining section to obtain flue gas, ash and coal slag respectively; the flue gas is mixed with the carbon dioxide generated by the calcination of limestone through the flue gas outlet, and high-concentration carbon dioxide is obtained after dust removal; the ash and coal slag are discharged from the coal slag outlet.
5. The method for producing cement by low carbon emission limestone muffle combustion according to claim 4, It is characterized in that The particle size of the crushed limestone particles is 7.5 mm to 15.0 mm, and the processing capacity is 5000 t / d to 6000 t / d.
6. The method for producing cement by low carbon emission limestone muffle combustion according to claim 4, It is characterized in that The preheating temperature is 750° C. to 870° C., and the preheating time is 5 min to 8 min.
7. The method for producing cement by low carbon emission limestone muffle combustion according to claim 4, It is characterized in that The calcination temperature is 1370° C. to 1450° C., and the calcination time is 12 min to 15 min.
8. The method for producing cement by low carbon emission limestone muffle combustion according to claim 4, It is characterized in that The cooling temperature is 900° C. to 930° C., and the cooling time is 8 min to 10 min.
9. The method for producing cement by low carbon emission limestone muffle combustion according to claim 4, It is characterized in that The amount of pulverized coal used is 200t / d~400t / d; the oxygen-coal ratio is 2.05~2.
15.
10. The method for producing cement by low carbon emission limestone muffle combustion according to claim 4, It is characterized in that After the carbon dioxide is discharged from the carbon dioxide outlet, it is dedusted by the dust removal device to obtain dust and carbon dioxide respectively; the dust is discharged from the dust outlet; the carbon dioxide enters the carbon dioxide collection unit; The dust removal efficiency is greater than or equal to 99%, and the dust concentration in the carbon dioxide after dust removal is less than 50mg / Nm 3 .