Amorphous alloy iron core capable of reducing stress on strip

By annealing and coating the epoxy resin adhesive layer during the production process of amorphous alloy cores, and applying mechanical vibration during the curing process, the stress problem of the strip is solved, the magnetic performance and stability are improved, and the application effect is improved.

CN118942831AInactive Publication Date: 2024-11-12HUNAN YANNENG SENYUAN ELECTRIC POWER EQUIP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410976889.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118942831A_ABST
    Figure CN118942831A_ABST
Patent Text Reader

Abstract

The invention discloses an amorphous alloy iron core capable of reducing the stress of a strip, and particularly relates to the technical field of amorphous alloy iron cores, the amorphous alloy iron core comprises an iron core ring, the outer side of the iron core ring is provided with a glue layer, and the glue layer is made of an epoxy resin material; comprising the following steps that firstly, an iron core ring is placed in an annealing furnace to be annealed, the annealing temperature is controlled to range from 375 DEG C to 380 DEG C, the heat preservation time ranges from 40 min to 75 min, in the annealing process, air in the annealing furnace is pumped out, and meanwhile nitrogen is inflated into the annealing furnace; 2, after annealing treatment is completed, the iron core ring is taken out and put into an environment full of nitrogen to be cooled; and 3, after cooling is completed, epoxy resin is adopted for coating the iron core ring, so that a layer of glue is formed on the outer wall of the iron core ring. In the production process, the stress on the strip can be reduced, so that the magnetic performance and the stability of the amorphous alloy iron core are guaranteed, the actual application effect of the amorphous alloy iron core is good, and the amorphous alloy iron core is convenient to popularize and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of amorphous alloy cores, and more particularly to an amorphous alloy core capable of reducing the stress of a strip. Background Art

[0002] The amorphous alloy core is a solid alloy obtained by ultra-rapid cooling solidification technology. It has a long-range disordered structure. Amorphous alloys (such as Nb-Ta-V) have the characteristics of high saturation magnetization, low coercive force, high remanence, excellent magnetic permeability, good oxidation resistance and high resistivity.

[0003] Although the amorphous alloy core in the prior art can be used normally, it still has many disadvantages in actual use. For example, the amorphous alloy core in the prior art cannot reduce the stress on the strip during the production process, which causes the magnetic properties and stability of the amorphous alloy core in the prior art to be easily affected. This results in the amorphous alloy core in the prior art and its production process not having good actual application effects, which is not conducive to promotion and use. Summary of the invention

[0004] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides an amorphous alloy core that can reduce the stress of the strip. The present invention can reduce the stress of the strip during the production process, so that the magnetic properties and stability of the amorphous alloy core are guaranteed. This makes the actual application effect of the present invention better and is easy to promote and use, so as to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above objectives, the present invention provides the following technical solutions: an amorphous alloy core capable of reducing the stress of a strip, comprising a core ring, a glue layer is arranged on the outer side of the core ring, and the glue layer is made of epoxy resin material.

[0006] A production process of an amorphous alloy core capable of reducing the stress of a strip, comprising the above-mentioned amorphous alloy core capable of reducing the stress of a strip and the following steps:

[0007] Step 1: Place the core ring in an annealing furnace for annealing, control the annealing temperature between 375-380°C, and keep it warm for 40-75 minutes. During the annealing process, extract the air in the annealing furnace and fill it with nitrogen at the same time;

[0008] Step 2: After the annealing treatment is completed, the core ring is taken out and placed in a nitrogen-filled environment for cooling;

[0009] Step 3: After cooling, the core ring is coated with epoxy resin to form a glue layer on the outer wall of the core ring;

[0010] Step 4: During the epoxy resin coating and curing process, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material during the process, while eliminating bubbles and improving the surface flatness of the coating layer;

[0011] Step 5: After coating, the finished amorphous alloy core is obtained.

[0012] In a preferred embodiment, the mechanical vibration frequency in step 4 is 0-5 kHz.

[0013] In a preferred embodiment, the mechanical vibration power in step 4 is 0.2-4 kW.

[0014] Technical effects and advantages of the present invention:

[0015] The invention comprises an iron core ring and a glue layer. In the production process, the iron core ring is first placed in an annealing furnace for annealing, and the annealing temperature is controlled between 375-380°C. The appropriate iron core annealing temperature should not only ensure the elimination of the internal stress of the iron core and restore its magnetic properties, but also reduce the brittleness of the amorphous alloy strip as much as possible. The heat preservation time is 40-75 minutes. In the annealing process, the air in the annealing furnace is extracted and nitrogen is filled into the annealing furnace at the same time, which can avoid the problem that the iron core ring is oxidized and the no-load loss increases. Then, after the annealing treatment is completed, the iron core ring is taken out and placed in a nitrogen-filled The invention is cooled in the environment. After the cooling is completed, the core ring is coated with epoxy resin so that a glue layer is formed on the outer wall of the core ring. During the coating and curing of the epoxy resin, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material in the process, and at the same time, bubbles are eliminated and the surface flatness of the coating layer is improved. After the coating is completed, the amorphous alloy core product is obtained. The invention can reduce the stress of the strip during the production process, so that the magnetic properties and stability of the amorphous alloy core are guaranteed, which makes the actual application effect of the invention better and is convenient for popularization and use. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the overall structure of the present invention.

[0017] Figure 2 It is a schematic diagram of the overall top-view cross-sectional structure of the present invention.

[0018] Figure 3 For the present invention Figure 2 Enlarged schematic diagram of the structure of part A in the middle.

[0019] The accompanying drawings are marked as follows: 1. core ring; 2. adhesive layer. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] As attached Figure 1 , Attachment Figure 2 and attached Figure 3 As shown, the present invention provides an amorphous alloy core capable of reducing the stress of a strip, comprising a core ring 1, a glue layer 2 is arranged on the outer side of the core ring 1, and the glue layer 2 is made of epoxy resin material.

[0023] A production process of an amorphous alloy core capable of reducing the stress of a strip, comprising the above-mentioned amorphous alloy core capable of reducing the stress of a strip and the following steps:

[0024] Step 1: placing the core ring 1 in an annealing furnace for annealing, controlling the annealing temperature to be between 380°C and the holding time to be 40 minutes. During the annealing process, the air in the annealing furnace is extracted and nitrogen is simultaneously filled into the annealing furnace;

[0025] Step 2: After the annealing treatment is completed, the core ring 1 is taken out and placed in an environment filled with nitrogen for cooling;

[0026] Step 3: After cooling, the core ring 1 is coated with epoxy resin so that a glue layer 2 is formed on the outer wall of the core ring 1;

[0027] Step 4: During the epoxy resin coating and curing process, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material during the process, while eliminating bubbles and improving the surface flatness of the coating layer;

[0028] Step 5: After coating, the finished amorphous alloy core is obtained.

[0029] The mechanical vibration frequency in step 4 is 5 kHz.

[0030] The mechanical vibration power in step 4 is 4 kW.

[0031] This embodiment can reduce the stress on the strip, so that the magnetic properties and stability of the amorphous alloy core are better than those of the prior art.

[0032] Example 2

[0033] As attached Figure 1 , Attachment Figure 2 and attached Figure 3 As shown, the present invention provides an amorphous alloy core capable of reducing the stress of a strip, comprising a core ring 1, a glue layer 2 is arranged on the outer side of the core ring 1, and the glue layer 2 is made of epoxy resin material.

[0034] A production process of an amorphous alloy core capable of reducing the stress of a strip, comprising the above-mentioned amorphous alloy core capable of reducing the stress of a strip and the following steps:

[0035] Step 1: placing the core ring 1 in an annealing furnace for annealing, controlling the annealing temperature to be between 380°C and the holding time to be 45 minutes. During the annealing process, the air in the annealing furnace is extracted and nitrogen is simultaneously filled into the annealing furnace;

[0036] Step 2: After the annealing treatment is completed, the core ring 1 is taken out and placed in an environment filled with nitrogen for cooling;

[0037] Step 3: After cooling, the core ring 1 is coated with epoxy resin so that a glue layer 2 is formed on the outer wall of the core ring 1;

[0038] Step 4: During the epoxy resin coating and curing process, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material during the process, while eliminating bubbles and improving the surface flatness of the coating layer;

[0039] Step 5: After coating, the finished amorphous alloy core is obtained.

[0040] The mechanical vibration frequency in step 4 is 4.5 kHz.

[0041] The mechanical vibration power in step 4 is 3.5 kW.

[0042] This embodiment can reduce the stress on the strip, so that the magnetic properties and stability of the amorphous alloy core are better than those of the prior art.

[0043] Example 3

[0044] As attached Figure 1 , Attachment Figure 2 and attached Figure 3 As shown, the present invention provides an amorphous alloy core capable of reducing the stress of a strip, comprising a core ring 1, a glue layer 2 is arranged on the outer side of the core ring 1, and the glue layer 2 is made of epoxy resin material.

[0045] A production process of an amorphous alloy core capable of reducing the stress of a strip, comprising the above-mentioned amorphous alloy core capable of reducing the stress of a strip and the following steps:

[0046] Step 1: placing the core ring 1 in an annealing furnace for annealing, controlling the annealing temperature between 375°C and the holding time for 70 minutes. During the annealing process, the air in the annealing furnace is extracted and nitrogen is filled into the annealing furnace at the same time;

[0047] Step 2: After the annealing treatment is completed, the core ring 1 is taken out and placed in an environment filled with nitrogen for cooling;

[0048] Step 3: After cooling, the core ring 1 is coated with epoxy resin so that a glue layer 2 is formed on the outer wall of the core ring 1;

[0049] Step 4: During the epoxy resin coating and curing process, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material during the process, while eliminating bubbles and improving the surface flatness of the coating layer;

[0050] Step 5: After coating, the finished amorphous alloy core is obtained.

[0051] The mechanical vibration frequency in step 4 is 5 kHz.

[0052] The mechanical vibration power in step 4 is 4 kW.

[0053] This embodiment can reduce the stress on the strip, so that the magnetic properties and stability of the amorphous alloy core are better than those of the prior art.

[0054] Example 4

[0055] As attached Figure 1 , Attachment Figure 2 and attached Figure 3 As shown, the present invention provides an amorphous alloy core capable of reducing the stress of a strip, comprising a core ring 1, a glue layer 2 is arranged on the outer side of the core ring 1, and the glue layer 2 is made of epoxy resin material.

[0056] A production process of an amorphous alloy core capable of reducing the stress of a strip, comprising the above-mentioned amorphous alloy core capable of reducing the stress of a strip and the following steps:

[0057] Step 1: placing the core ring 1 in an annealing furnace for annealing, controlling the annealing temperature between 375°C and the holding time for 75 minutes. During the annealing process, the air in the annealing furnace is extracted and nitrogen is filled into the annealing furnace at the same time;

[0058] Step 2: After the annealing treatment is completed, the core ring 1 is taken out and placed in an environment filled with nitrogen for cooling;

[0059] Step 3: After cooling, the core ring 1 is coated with epoxy resin so that a glue layer 2 is formed on the outer wall of the core ring 1;

[0060] Step 4: During the epoxy resin coating and curing process, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material during the process, while eliminating bubbles and improving the surface flatness of the coating layer;

[0061] Step 5: After coating, the finished amorphous alloy core is obtained.

[0062] The mechanical vibration frequency in step 4 is 4.5 kHz.

[0063] The mechanical vibration power in step 4 is 3.5 kW.

[0064] This embodiment can reduce the stress on the strip, so that the magnetic properties and stability of the amorphous alloy core are better than those of the prior art.

[0065] The present invention comprises an iron core ring 1 and a glue layer 2. In the production process, the iron core ring 1 is first placed in an annealing furnace for annealing, and the annealing temperature is controlled between 375-380°C. The appropriate iron core annealing temperature should not only ensure the elimination of the internal stress of the iron core and restore its magnetic properties, but also reduce the brittleness of the amorphous alloy strip as much as possible. The heat preservation time is 40-75 minutes. During the annealing process, the air in the annealing furnace is extracted and nitrogen is filled into the annealing furnace at the same time, which can avoid the iron core ring 1 from being oxidized, resulting in an increase in no-load loss. Then, after the annealing treatment is completed, the iron core ring 1 is taken out and placed in a nitrogen-filled furnace. The iron core ring 1 is cooled in an environment, and after the cooling is completed, the iron core ring 1 is coated with epoxy resin so that a glue layer 2 is formed on the outer wall of the iron core ring 1. During the coating and curing of the epoxy resin, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material, while eliminating bubbles and improving the surface flatness of the coating layer. After the coating is completed, an amorphous alloy core product is obtained. The present invention can reduce the stress on the strip during the production process, so that the magnetic properties and stability of the amorphous alloy core are guaranteed, which makes the actual application effect of the present invention better and is convenient for popularization and use.

[0066] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An amorphous alloy core capable of reducing the stress of a strip, comprising a core ring (1), Features: A glue layer (2) is provided on the outer side of the core ring (1), and the glue layer (2) is made of epoxy resin material.

2. A production process for an amorphous alloy core capable of reducing the stress of a strip, It is characterized in that The invention comprises an amorphous alloy core capable of reducing the stress of a strip as claimed in claim 1 and the following steps: Step 1: placing the core ring (1) in an annealing furnace for annealing, controlling the annealing temperature to be between 375° C. and 380° C., and holding the temperature for 40 to 75 minutes. During the annealing process, the air in the annealing furnace is evacuated, and nitrogen is simultaneously introduced into the annealing furnace; Step 2: After the annealing treatment is completed, the core ring (1) is taken out and placed in a nitrogen-filled environment for cooling; Step 3: After cooling, the core ring (1) is coated with epoxy resin so that a glue layer (2) is formed on the outer wall of the core ring (1); Step 4: During the epoxy resin coating and curing process, a magnetostrictive transducer is used to apply mechanical vibration to reduce the internal stress caused by the volume shrinkage of the thermoplastic material during the process, while eliminating bubbles and improving the surface flatness of the coating layer; Step 5: After coating, the finished amorphous alloy core is obtained.

3. The production process of an amorphous alloy core capable of reducing the stress of a strip according to claim 1, Features: The mechanical vibration frequency in step 4 is 0-5kHz.

4. The amorphous alloy core capable of reducing the stress of the strip according to claim 1, Features: The mechanical vibration power in step 4 is 0.2-4kW.

Citation Information

Patent Citations

  • Curing method for reducing internal stress of amorphous iron core

    CN106128746A

  • Production process of PFC differential mode inductance magnetic ring

    CN111584226A

  • Amorphous alloy ribbon

    JP2006045662A

  • Iron-based amorphous alloy having low stress sensitivity, and preparation method therefor

    US20190256944A1