NiMoP electrode material and preparation method and application thereof

By adjusting the ratio of nickel, molybdenum and phosphorus and hydrothermal conditions, NiMoP electrode material with high specific surface area was prepared, which solved the problems of low capacity and insufficient electrochemical performance of nickel-based phosphide electrode material, and significantly improved its in supercapacitors electrochemical properties.

CN118942921APending Publication Date: 2024-11-12QIQIHAR UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411312949.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing nickel-based phosphide electrode materials have problems with low capacity and insufficient conductivity and rate performance in supercapacitors, which affect their electrochemical performance.

Method used

By mixing soluble nickel salt, molybdenum source and phosphate with water for hydrothermal reaction, nickel-molybdenum-based phosphate, then baking to prepare NiMoP electrode material, adjust the ratio of nickel element to phosphate and molybdenum source, and control the hydrothermal heat Through reaction temperature and time, NiMoP electrode material with uniform morphology and high specific surface area was prepared.

Benefits of technology

Improves the electrochemical performance of NiMoP electrode materials, including faster redox reaction rates and greater charge storage capabilities, extends discharge time and expands the voltage window.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942921A_ABST
    Figure CN118942921A_ABST
Patent Text Reader

Abstract

The invention provides a NiMoP electrode material and a preparation method and application thereof, and relates to the technical field of supercapacitors. The invention provides a preparation method of a NiMoP electrode material, which comprises the following steps: mixing soluble nickel salt, a soluble molybdenum source, soluble phosphate, a conductive substrate and water for hydrothermal reaction to obtain nickel-molybdenum-based phosphate; and roasting the nickel-molybdenum-based phosphate to generate nickel-molybdenum phosphide, so as to obtain the NiMoP electrode material. The ratio of the amount of substance of a nickel element in the soluble nickel salt to the amount of substance of a phosphorus element in the soluble phosphate is 1: (1-8); the ratio of the amount of substance of the nickel element in the soluble nickel salt to the amount of substance of the molybdenum element in the soluble molybdenum source is 1: 1; the temperature of the hydrothermal reaction is 100-180 DEG C, and the time is 3-15 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of supercapacitors, and in particular to a NiMoP electrode material and a preparation method and application thereof. Background Art

[0002] Supercapacitors have the advantages of high power density and long cycle life, meeting the great demand of modern society for new energy devices. Electrode materials are the most important component of supercapacitors. Proven high-performance electrode materials include nickel-phosphorus and cobalt-phosphorus, based on Ni 2+ / Ni 3+ The conversion and α-CoOOH / β-CoOOH phase transition reaction of different crystal phases. Compared with transition metal oxides, transition metal phosphides are metallic compounds with rich valence states due to the existence of electron orbits, and the electronegativity of phosphorus atoms is less than that of oxygen atoms, so they have higher conductivity.

[0003] Among them, nickel-based phosphides are very ideal electrode materials with the advantages of high electrochemical activity and low cost. Metal bonds and covalent bonds coexist in nickel phosphide. On the one hand, Ni(II) bound by covalent bonds in nickel phosphide stores charge through Faraday reaction to provide high capacitance. On the other hand, Ni bound by metal bonds provides free electrons to improve conductivity. However, in terms of practical applications, nickel-based phosphides also have the problem of low capacity. Therefore, researchers began to explore the construction and application of bimetallic phosphides. Among them, Ni-Co-P shows better charge storage properties than single metal phosphides. Because of the mutual synergy of multiple metals, richer redox reactions are brought about, such as: nickel cobalt phosphides with multiple valence states can prolong the discharge time, expand the voltage window, and thus improve the specific capacity. Despite these advantages, its electrochemical properties such as conductivity and rate performance still need to be further improved. Summary of the invention

[0004] In view of this, an object of the present invention is to provide a NiMoP electrode material and a preparation method and application thereof. The NiMoP electrode material provided by the present invention has good electrochemical properties.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a NiMoP electrode material, comprising the following steps:

[0007] A soluble nickel salt, a soluble molybdenum source, a soluble phosphate, a conductive substrate and water are mixed for hydrothermal reaction to obtain a nickel-molybdenum-based phosphate;

[0008] The nickel-molybdenum-based phosphate is calcined to generate nickel-molybdenum phosphide to obtain the NiMoP electrode material;

[0009] The ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:1-8;

[0010] The ratio of the amount of nickel in the soluble nickel salt to the amount of molybdenum in the soluble molybdenum source is 1:1;

[0011] The temperature of the hydrothermal reaction is 100-180° C., and the time is 3-15 hours.

[0012] Preferably, the soluble nickel salt includes one or more of nickel acetate, nickel nitrate and nickel sulfate.

[0013] Preferably, the soluble molybdenum source includes one or more of sodium molybdate, ammonium molybdate and molybdic acid.

[0014] Preferably, the soluble phosphate includes one or more of sodium hypophosphite, sodium dihydrogen phosphate and potassium dihydrogen phosphate.

[0015] Preferably, the ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:5;

[0016] The temperature of the hydrothermal reaction is 160° C. and the time is 12 h.

[0017] Preferably, the calcination temperature is 300-600° C. and the calcination time is 1-6 hours.

[0018] The present invention also provides a NiMoP electrode material prepared by the preparation method described in the above technical solution, wherein the NiMoP is loaded on a conductive substrate, and the shape of the NiMoP includes spherical and / or flake.

[0019] Preferably, the loading amount of NiMoP is 1.1 to 1.8 mg·cm -2 .

[0020] Preferably, when the NiMoP is spherical, the diameter of the NiMoP is 1-2 μm; when the NiMoP is flake-shaped, the length of the NiMoP is 1-3 μm; and the thickness is 50-200 nm.

[0021] The present invention also provides the application of the NiMoP electrode material described in the above technical solution in a supercapacitor.

[0022] The present invention provides a method for preparing a NiMoP electrode material, comprising the following steps:

[0023] A soluble nickel salt, a soluble molybdenum source, a soluble phosphate, foamed nickel and water are mixed for hydrothermal reaction to obtain nickel-molybdenum-based phosphate;

[0024] The nickel-molybdenum-based phosphate is calcined to generate nickel-molybdenum phosphide to obtain the NiMoP electrode material;

[0025] The ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:1-8;

[0026] The ratio of the amount of nickel in the soluble nickel salt to the amount of molybdenum in the soluble molybdenum source is 1:1;

[0027] The temperature of the hydrothermal reaction is 100-180° C., and the time is 3-15 hours.

[0028] The present invention prepares a NiMoP electrode material with uniform morphology and high specific surface area by adjusting the ratio of the amount of nickel element in a soluble nickel salt to the amount of phosphorus element in a soluble phosphate, the ratio of the amount of nickel element in a soluble nickel salt to the amount of molybdenum element in a soluble molybdenum source, and the temperature and time of a hydrothermal reaction; the NiMoP electrode material with uniform morphology and high specific surface area has excellent porosity, is conducive to electrolyte penetration, can effectively shorten the transmission path of ions inside the electrode material, thereby improving the reaction rate of the electrode material; and the NiMoP electrode with a high specific surface area can provide more active sites for redox reactions, accelerate the redox reaction rate, and further improve the electrochemical performance of the electrode material.

[0029] Furthermore, when the ratio of the amount of nickel element in the soluble nickel salt to the amount of phosphorus element in the soluble phosphate is 1:5, the temperature of the hydrothermal reaction is 160°C, and the time is 12 hours, the morphology of the NiMoP electrode material is more uniform and the specific surface area is larger, thereby improving the electrochemical performance of the electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is the XRD pattern of NiMoP-5 in Example 3;

[0031] Figure 2 This is the test result diagram of NiMoP-5 specific surface area and pore size distribution;

[0032] Figure 3 SEM images of NiMoP-1 at different magnifications;

[0033] Figure 4 The SEM images of NiMoP-3 at different magnifications;

[0034] Figure 5SEM images of NiMoP-5 at different magnifications;

[0035] Figure 6 The SEM images of NiMoP-8 at different magnifications;

[0036] Figure 7 This is a graph showing the electrochemical performance test results of NiMoP-1;

[0037] Figure 8 This is a graph showing the electrochemical performance test results of NiMoP-3;

[0038] Fig. 9 This is a graph showing the electrochemical performance test results of NiMoP-5;

[0039] Fig.10 This is a graph showing the electrochemical performance test results of NiMoP-8;

[0040] Fig.11 The SEM images of NiMoP-5-3 at different magnifications;

[0041] Fig.12 The SEM images of NiMoP-5-9 at different magnifications;

[0042] Fig.13 The SEM images of NiMoP-5-15 at different magnifications;

[0043] Fig.14 This is a graph showing the electrochemical performance test results of NiMoP-5-3;

[0044] Fig.15 This is a graph showing the electrochemical performance test results of NiMoP-5-6;

[0045] Fig.16 This is a graph showing the electrochemical performance test results of NiMoP-5-9;

[0046] Fig.17 This is a graph showing the electrochemical performance test results of NiMoP-5-12;

[0047] Fig.18 This is a graph showing the electrochemical performance test results of NiMoP-5-15;

[0048] Fig.19 This is a comparison chart of the electrochemical performance of the electrode materials prepared in Examples 5 to 9 under the same test conditions;

[0049] Fig. 20 This is a graph showing the electrochemical performance test results of NiMoP-5-100;

[0050] Fig.21This is a graph showing the electrochemical performance test results of NiMoP-5-130;

[0051] Fig. 22 This is a graph showing the electrochemical performance test results of NiMoP-5-160;

[0052] Fig.23 This is a graph showing the electrochemical performance test results of NiMoP-5-180;

[0053] Fig.24 This is a comparison chart of the electrochemical performance of the electrode materials prepared in Examples 10 to 13 under the same test conditions. DETAILED DESCRIPTION

[0054] The present invention provides a method for preparing a NiMoP electrode material, comprising the following steps:

[0055] A soluble nickel salt, a soluble molybdenum source, a soluble phosphate, a foamed nickel and water are mixed for hydrothermal reaction and then the obtained solid phase is roasted to obtain the NiMoP electrode material;

[0056] The ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:1-8;

[0057] The ratio of the amount of nickel in the soluble nickel salt to the amount of molybdenum in the soluble molybdenum source is 1:1;

[0058] The temperature of the hydrothermal reaction is 100-180° C., and the time is 3-15 hours.

[0059] In the present invention, the ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:1-8. In a specific embodiment, the ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7 or 1:8. In the present invention, the soluble nickel salt preferably includes one or more of nickel acetate, nickel nitrate and nickel sulfate; the soluble phosphate preferably includes one or more of sodium hypophosphite, sodium dihydrogen phosphate and potassium dihydrogen phosphate.

[0060] In the present invention, the ratio of the amount of nickel in the soluble nickel salt to the amount of molybdenum in the soluble molybdenum source is 1: 1. In the present invention, the soluble molybdenum source preferably includes one or more of sodium molybdate, ammonium molybdate and molybdic acid.

[0061] In the present invention, the ratio of the amount of nickel element in the soluble nickel salt to the volume of water is preferably 1 mmol:30-150 mL. In a specific embodiment, the ratio of the amount of nickel element in the soluble nickel salt to the volume of water can be 1 mmol:30 mL, 2 mmol:60 mL, 3 mmol:90 mL, 4 mmol:120 mL or 5 mmol:150 mL.

[0062] In the present invention, the conductive base material preferably includes one or more of foamed nickel, foamed copper, carbon cloth and carbon paper.

[0063] In the present invention, the temperature of the hydrothermal reaction is 100-180° C., and in a specific embodiment, the temperature of the hydrothermal reaction can be 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C. or 180° C. In the present invention, the time of the hydrothermal reaction is 3-15 hours, and in a specific embodiment, the time of the hydrothermal reaction can be 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours or 15 hours.

[0064] After the hydrothermal reaction, the present invention preferably performs solid-liquid separation on the product obtained by the hydrothermal reaction, and then washes and dries the obtained wet solid phase to obtain a solid phase.

[0065] In the present invention, the detergent used for the washing preferably includes anhydrous ethanol and distilled water. The washing is preferably performed under centrifugal conditions.

[0066] After the hydrothermal reaction, black powder of nickel-molybdenum-based phosphate was formed.

[0067] In the present invention, the calcination temperature is preferably 100-600°C. In a specific embodiment, the calcination temperature can be 100°C, 200°C, 300°C, 400°C, 500°C or 600°C. The time is preferably 1-6h. In a specific embodiment, the calcination time can be 1h, 2h, 3h, 4h, 5h or 6h.

[0068] In the present invention, the calcination is preferably carried out in a protective atmosphere; the gas in the protective atmosphere preferably includes nitrogen.

[0069] The present invention also provides a NiMoP electrode material prepared by the preparation method described in the above technical solution, wherein the NiMoP is loaded on a conductive substrate material, and the shape of the NiMoP includes spherical and / or flake.

[0070] In the present invention, the loading amount of NiMoP is preferably 1.1 to 1.8 mg·cm -2When the NiMoP is spherical, the diameter of the NiMoP is preferably 1 to 2 μm; when the NiMoP is flake-shaped, the length of the NiMoP is preferably 1 to 3 μm; and the thickness is preferably 50 to 200 nm.

[0071] The present invention also provides the application of the NiMoP electrode material described in the above technical solution in a supercapacitor.

[0072] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0073] Example 1

[0074] Nickel foam processing:

[0075] First, nickel foam (1.5mm*200mm*250mm, surface density: 350g / m 3 PPI110, pore size: 0.1 mm, porosity: 97.2%) cut into an area of ​​2×3 cm 2 The resulting samples were ultrasonically treated in 1 M hydrochloric acid, acetone and deionized water, respectively, and then dried in an oven at 60 °C for 12 h.

[0076] Weigh 1mmol nickel acetate, 1mmol sodium molybdate and 1mmol sodium hypophosphite into a 50mL beaker, add 30mL of distilled water and stir until completely dissolved, then transfer to the reactor and add a 2×3cm treated piece of 2 The nickel foam was subjected to a hydrothermal reaction (reaction temperature was 160°C and reaction time was 12h). After the reaction, the prepared powder sample was repeatedly centrifuged and washed three times with anhydrous ethanol and distilled water, and the nickel foam substrate on which the NiMoP was grown in situ was rinsed with double distilled water. The electrode material prepared above was dried at 80°C for 12h, and calcined at 400°C for 2h in a tube furnace under a N2 protective atmosphere. The obtained sample was recorded as NiMoP-1.

[0077] Example 2

[0078] The only difference from Example 1 is that the amount of sodium hypophosphite used is 3 mmol; the obtained sample is recorded as NiMoP-3.

[0079] Example 3

[0080] The only difference from Example 1 is that the amount of sodium hypophosphite used is 5 mmol; the obtained sample is recorded as NiMoP-5.

[0081] Example 4

[0082] The only difference from Example 1 is that the amount of sodium hypophosphite used is 8 mmol; the obtained sample is recorded as NiMoP-8.

[0083] The loading amounts of active materials for NiMoP-1, NiMoP-3, NiMoP-5, and NiMoP-8 are approximately 1.5 mg cm -2 , 1.4mg·cm -2 、1.8mg·cm -2 and 1.3 mg cm -2 .

[0084] The NiMoP in the NiMoP-5 in Example 3 was peeled off from the nickel foam and then subjected to XRD analysis. The results are as follows: Figure 1 shown.

[0085] Depend on Figure 1 It can be seen that the characteristic diffraction peaks of NiMoP basically match the characteristic peaks of the crystal structure of MoNiP8 (JCPDS card No. 50-1191), which shows that the prepared NiMoP material is a MoNiP8 electrode material. The eight significant characteristic diffraction peaks of the MoNiP8 material at 2θ of 19.3°, 26.2°, 28.6°, 34.9°, 49.2°, 50.9°, 59.0° and 65.9° correspond to the (101), (102), (110), (103), (212), (114), (220) and (312) crystal planes of MoNiP8, respectively. It can be seen that the prepared NiMoP material is MoNiP8.

[0086] The specific surface area and pore size distribution of NiMoP-5 were tested. The results are as follows: Figure 2 As shown. Among them, Figure 2 (a) is the nitrogen adsorption-desorption curve of NiMoP-5; Figure 2 (b) is the pore size distribution curve of NiMoP-5

[0087] Depend on Figure 2 It can be seen that the nitrogen adsorption-desorption curve of NiMoP-5 shows a type IV isotherm with an obvious hysteresis loop, indicating that NiMoP-5 has typical mesoporous characteristics. The specific surface area of ​​NiMoP-5 calculated by the BET method is 106.5m 2 / g, through Figure 2 From the pore size distribution curve (b), it can be seen that the porosity of the NiMoP electrode material is evenly distributed, and the central pore diameter is approximately 10 nm.

[0088] SEM analysis of NiMoP-1 was performed at different magnifications. Figure 3 As shown. Among them, Figure 3 (a) is the SEM image of NiMoP-1 with a scale of 1 μm; Figure 3 (b) is the SEM image of NiMoP-1 with a scale of 500 nm.

[0089] Depend on Figure 3 It can be seen that when Ni:P=1:1, the prepared electrode material has a spherical structure. Figure 3 In (a), it can be observed that the microspheres stick together to form microsphere clusters. Figure 3 As can be observed in (b), the diameter of the microsphere is about 2 μm. It is composed of stacked short nanorods, and a large number of worm-like nanorods can be observed on its surface.

[0090] SEM analysis of NiMoP-3 was performed at different magnifications. The results are as follows: Figure 4 As shown. Among them, Figure 4 (a) is the SEM image of NiMoP-3 with a scale of 1 μm; Figure 4 (b) is the SEM image of NiMoP-3 with a scale of 500nm.

[0091] Depend on Figure 4 It can be seen that when Ni:P=1:3, the prepared electrode material is composed of a mixture of microspheres and nanosheets, and the microspheres are more than the nanosheets. The microspheres and nanosheets are adhered to each other, and the diameter of the microspheres is about 1μm. This shows that with the increase of the Ni:P molar ratio, the morphology of the electrode material gradually evolves from microspheres to nanosheets.

[0092] SEM analysis of NiMoP-5 was performed at different magnifications. Figure 5 As shown. Among them, Figure 5 (a) is the SEM image of NiMoP-5 with a scale of 1 μm; Figure 5 (b) is the SEM image of NiMoP-5 with a scale of 500 nm.

[0093] Depend on Figure 5 It can be seen that when the molar ratio Ni:P=1:5, the prepared electrode material has a nanosheet structure, the nanosheets are staggeredly grown on the conductive substrate nickel foam and have a smooth surface, the width of the nanosheet is about 3 μm, and the thickness is about 200 nm.

[0094] SEM analysis of NiMoP-8 was performed at different magnifications. The results are as follows: Figure 6 shown. Figure 6 The SEM images of NiMoP-8 at different magnifications are shown below. Figure 6 (a) is the SEM image of NiMoP-8 with a scale of 1 μm; Figure 6(b) is the SEM image of NiMoP-8 with a scale of 500 nm.

[0095] Depend on Figure 6 It can be seen that when the molar ratio of Ni:P=1:8, the morphology of the prepared electrode material is still a nanosheet structure, but the thickness of the nanosheet becomes thinner, and a small amount of nanosheets are cracked to form a nanorod structure. At the same time, the width of the nanosheet is about 1μm and the thickness is about 50nm. It can be seen that as the molar ratio of Ni:P increases, the thickness of the nanosheet gradually becomes thinner.

[0096] The electrochemical performance of NiMoP-1 was tested, and the results are as follows Figure 7 As shown. Among them, Figure 7 (a) shows the CV curves of NiMoP-1 at different scan rates; Figure 7 (b) is the charge-discharge curve of NiMoP-1 at different current densities. The oxidation peaks at different scan rates obtained from the CV curves are shown in Table 1, and the specific capacity results at different current densities calculated from the charge-discharge curves are shown in Table 2.

[0097] Depend on Figure 7 As shown in (a), a pair of obvious redox peaks appear in the CV curve, indicating that the electrode material undergoes a redox reaction during the charge transfer process, indicating that the electrochemical behavior of the NiMoP material is pseudocapacitive behavior. As the scan rate increases, the oxidation peak and reduction peak in the CV curve move to the two ends of the potential, which is caused by the resistance and polarization of the electrode itself.

[0098] Depend on Figure 7 As can be seen in (b), the charge and discharge curves of NiMoP-1 at different current densities show obvious charge and discharge platforms, indicating that the prepared NiMoP-1 is a battery-type electrode material.

[0099] The electrochemical performance of NiMoP-3 was tested, and the results are as follows Figure 8 As shown. Among them, Figure 8 (a) shows the CV curves of NiMoP-3 at different scan rates; Figure 8 (b) is the charge and discharge curve of NiMoP-3 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 1, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 2.

[0100] Depend on Figure 8 As shown in (a), a pair of obvious redox peaks appear in the CV curves of the NiMoP-3 electrode material, indicating that the electrode material undergoes a redox reaction during the charge transfer process, indicating that the electrochemical behavior of the NiMoP material is a pseudocapacitive behavior.

[0101] Depend on Figure 8 As can be seen in (b), the charge and discharge curve is almost symmetrical and nonlinear, indicating that the NiMoP-3 electrode has a good coulombic efficiency.

[0102] The electrochemical performance of NiMoP-5 was tested, and the results are as follows Fig. 9 As shown. Among them, Fig. 9 (a) shows the CV curves of NiMoP-5 at different scan rates; Fig. 9 (b) is the charge and discharge curve of NiMoP-5 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 1, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 2.

[0103] Depend on Fig. 9 As shown in (a), a pair of obvious redox peaks appear in the CV curves of the NiMoP-5 electrode material, indicating that a redox reaction occurs during the charge transfer process, indicating that the electrochemical behavior of the NiMoP-5 material is a pseudocapacitive behavior.

[0104] The electrochemical performance of NiMoP-8 was tested, and the results are as follows Fig.10 As shown. Among them, Fig.10 (a) shows the CV curves of NiMoP-8 at different scan rates; Fig.10 (b) is the charge and discharge curve of NiMoP-8 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 1, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 2.

[0105] Depend on Fig.10 As shown in (a), with the continuous increase of the scanning rate, the oxidation peak of the CV curve gradually increases, and the integral area of ​​the CV curve also gradually increases.

[0106] from Figures 7-10 In (b), it can be observed that the charge and discharge curves of all electrode materials have an obvious discharge platform, and the voltage value corresponding to the platform is about 0.4V, which is a typical battery-type electrode material. When the current density increases from 1A / g to 10A / g, the discharge time of the electrode material is significantly shortened and the specific capacity is reduced. This may be because at high current density, the electrode material fails to fully participate in the redox reaction and begins to discharge.

[0107] Table 1 Oxidation peak values ​​(V) of NiMoP materials prepared with different molar ratios at different scanning rates

[0108] 1mV / s 2mV / s 3mV / s 4mV / s 5mV / s 6mV / s 7mV / s 8mV / s 9mV / s 10mV / s NiMoP-1 0.443 0.463 0.473 0.481 0.488 0.493 0.498 0.504 0.508 0.512 NiMoP-3 0.485 0.496 0.504 0.511 0.517 0.521 0.526 0.531 0.531 0.540 NiMoP-5 0.499 0.517 0.521 0.534 0.547 0.560 0.552 0.561 0.554 0.558 NiMoP-8 0.495 0.505 0.513 0.519 0.527 0.532 0.534 0.537 0540 0.543

[0109] Table 2 Specific capacity (mAh / g) of NiMoP materials prepared with different molar ratios at different current densities

[0110] 1A / g 3A / g 5A / g 7A / g 9A / g 10A / g NiMoP-1 190.4 180.8 172.1 166.1 160.1 158.9 NiMoP-3 298.6 257.7 245.9 240.5 236.5 234.7 NiMoP-5 331.7 293.3 277.2 217.8 210.7 205.3 NiMoP-8 206.9 187.9 175.8 169.8 164.8 162.5

[0111] Example 5

[0112] Weigh 1.2445 g (5 mmol) nickel acetate, 1.2096 g (5 mmol) sodium molybdate, and 2.6502 g (25 mmol) sodium hypophosphite into a beaker (nNi:nMo:nP = 1:1:5), add 150 mL of distilled water and stir until completely dissolved, then evenly load into 5 reactors of the same volume, and add a 2*3 cm2 piece of the treated carbonyl phosphate in Example 1 into one of the reactors. 2 The nickel foam was subjected to a hydrothermal reaction (reaction temperature was 160°C, reaction time was 3h). After the reaction, the obtained powder was centrifugally washed 3 times with anhydrous ethanol and distilled water, and the nickel foam with in-situ growth of NiMoP was rinsed with distilled water for many times. The electrode material prepared above was dried at 80°C for 12h, and finally calcined at 400°C for 2h in a tube furnace under N2 protective atmosphere. The obtained sample was recorded as NiMoP-5-3.

[0113] Example 6

[0114] The only difference from Example 5 is that the reaction time is 6 h; the obtained sample is recorded as NiMoP-5-6.

[0115] Example 7

[0116] The only difference from Example 5 is that the reaction time is 9 h; the obtained sample is recorded as NiMoP-5-9.

[0117] Example 8

[0118] The only difference from Example 5 is that the reaction time is 12 h; the obtained sample is recorded as NiMoP-5-12.

[0119] Example 9

[0120] The only difference from Example 5 is that the reaction time is 15 h; the obtained sample is recorded as NiMoP-5-15.

[0121] The loading amounts of active materials for NiMoP-5-3, NiMoP-5-6, NiMoP-5-9, NiMoP-5-12, and NiMoP-5-15 were approximately 1.2 mg cm -2 , 1.5mg·cm -2 , 1.7mg·cm -2 , 1.4mg·cm -2 and 1.3 mg cm-2 .

[0122] SEM analysis of NiMoP-5-3 was performed at different magnifications. The results are as follows: Fig.11 As shown. Among them, Fig.11 (a) is the SEM image of NiMoP-5-3 with a scale of 1 μm; Fig.11 (b) is the SEM image of NiMoP-5-3 with a scale of 500 nm.

[0123] from Fig.11 It can be seen that the morphological features of NiMoP-5-3 are mostly spherical structures, with only a small amount of lamellar structures formed.

[0124] SEM analysis of NiMoP-5-9 was performed at different magnifications. The results are as follows: Fig.12 As shown. Among them, Fig.12 (a) is the SEM image of NiMoP-5-9 with a scale of 1 μm; Fig.12 (b) is the SEM image of NiMoP-5-9 with a scale of 500 nm.

[0125] from Fig.12 It can be seen that with the increase of phosphating time, when the reaction time is 9h, the morphology of the electrode material has evolved into a lamellar structure, and the surface of the nanosheet is smooth and the morphology is uniform. The width of the nanosheet is about 1μm and the thickness is about 100nm.

[0126] SEM analysis of NiMoP-5-15 was performed at different magnifications. The results are as follows: Fig.13 As shown. Among them, Fig.13 (a) is the SEM image of NiMoP-5-15 with a scale of 1 μm; Fig.13 (b) is the SEM image of NiMoP-5-15 with a scale of 500 nm.

[0127] from Fig.13 It can be seen that as the phosphating time continues to increase, when the reaction time is 15h, the sheet-like electrode materials collapse and stack, adhering to each other to form an irregular shape.

[0128] The electrochemical performance of NiMoP-5-3 was tested, and the results are as follows Fig.14 As shown. Among them, Fig.14 (a) shows the CV curves of NiMoP-5-3 at different scan rates; Fig.14 (b) is the charge and discharge curve of NiMoP-5-3 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 3, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 4.

[0129] The electrochemical performance of NiMoP-5-6 was tested, and the results are as follows Fig.15 As shown. Among them, Fig.15 (a) shows the CV curves of NiMoP-5-6 at different scan rates; Fig.15 (b) is the charge and discharge curve of NiMoP-5-6 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 3, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 4.

[0130] The electrochemical performance of NiMoP-5-9 was tested, and the results are as follows Fig.16 As shown. Among them, Fig.16 (a) shows the CV curves of NiMoP-5-9 at different scan rates; Fig.16 (b) is the charge and discharge curve of NiMoP-5-9 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 3, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 4.

[0131] The electrochemical performance of NiMoP-5-12 was tested, and the results are as follows Fig.17 As shown. Among them, Fig.17 (a) shows the CV curves of NiMoP-5-12 at different scan rates; Fig.17 (b) is the charge and discharge curve of NiMoP-5-12 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 3, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 4.

[0132] The electrochemical performance of NiMoP-5-15 was tested, and the results are as follows Fig.18 As shown. Among them, Fig.18 (a) shows the CV curves of NiMoP-5-15 at different scan rates; Fig.18 (b) is the charge and discharge curve of NiMoP-5-15 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 3, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 4.

[0133] Depend on Figures 14 to 18 As shown in (a), a pair of obvious redox peaks appear in the CV curve, indicating that the electrode material undergoes a redox reaction during the charge transfer process, indicating that the energy storage behavior of the electrode material is pseudocapacitive behavior. It can be observed from the figure that as the scan rate increases, the oxidation peak and reduction peak in the CV curve move toward the potential boundary, which is caused by the resistance and polarization of the electrode itself.

[0134] Depend on Figures 14 to 18 As shown in (b), the charge and discharge curves of all electrode materials have obvious discharge platforms, which are typical battery-type materials. When the current density increases from 1A / g to 10A / g, the charge and discharge time of the electrode material is significantly shortened. This may be because under high current density conditions, the electrode active material fails to fully participate in the redox reaction, and the low ion diffusion rate cannot meet the rapid redox reaction under high current density, resulting in low utilization of the electrode material. Its charge and discharge curve is a symmetrical nonlinear relationship, indicating that the electrode has good chemical reversibility.

[0135] Fig.19 : is a comparison diagram of the electrochemical performance of the electrode materials prepared in Examples 5 to 9 under the same test conditions. Among them, the CV comparison curves of the electrode materials prepared in Examples 5 to 9 at a scan rate of 6 mV / s are as follows: Fig.19 As shown in (a), the charge and discharge comparison curves of the electrode materials prepared at different times at a current density of 1A / g are as follows Fig.19 As shown in (b).

[0136] Depend on Fig.19 (a) It can be seen that at the same scan rate, the CV integrated area of ​​the NiMoP-5-12 electrode material prepared with a reaction time of 12 h is the largest, and the peak current is the largest. Fig.19 (b) It can be seen that the coulombic efficiency of the charge and discharge curve of NiMoP-5-12 is the largest and the discharge time is the longest.

[0137] Table 3 Oxidation peak values ​​(V) of NiMoP materials prepared at different times at different scanning rates

[0138] 1mV / s 2mV / s 3mV / s 4mV / s 5mV / s 6mV / s 7mV / s 8mV / s 9mV / s 10mV / s NiMoP-5-3 0.498 0.511 0.519 0.518 0.522 0.526 0.528 0.531 0.534 0.535 NiMoP-5-6 0.514 0.528 0.538 0.548 0.553 0.559 0.566 0.571 0.576 0.582 NiMoP-5-9 0.496 0.522 0.540 0.547 0.550 0.556 0.558 0.563 0.568 0.571 NiMoP-5-12 0.499 0.517 0.521 0.534 0.547 0.560 0.552 0.561 0.554 0.558 NiMoP-5-15 0.505 0.516 0.520 0.534 0.541 0.545 0.549 0.552 0.557 0.559

[0139] Table 4 Specific capacity (mAh / g) of NiMoP materials prepared at different times at different current densities

[0140]

[0141]

[0142] Example 10

[0143] Weigh 1.4929 g (4 mmol) of nickel acetate, 1.4518 g (4 mmol) of sodium molybdate and 3.1880 g (20 mmol) of sodium hypophosphite into a beaker, add 120 mL of distilled water and stir until completely dissolved, then add them evenly into 4 reactors of the same volume, and add a 2×3 cm2 piece of the treated carbonyl phosphate in Example 1 into one of the reactors. 2The nickel foam was subjected to a hydrothermal reaction (reaction time was 12 h, reaction temperature was 100° C.) and the prepared nickel foam was rinsed with double distilled water. The electrode material prepared above was dried at 80° C. for 12 h, and calcined at 400° C. for 2 h in a tube furnace under a N2 protective atmosphere. The obtained sample was recorded as NiMoP-5-100.

[0144] Embodiment 11

[0145] The only difference from Example 10 is that the reaction temperature is 130°C; the obtained sample is recorded as NiMoP-5-130.

[0146] Example 12

[0147] The only difference from Example 5 is that the reaction temperature is 160°C; the obtained sample is recorded as NiMoP-5-160.

[0148] Example 13

[0149] The only difference from Example 5 is that the reaction temperature is 180°C; the obtained sample is recorded as NiMoP-5-180.

[0150] The loading amounts of active materials for NiMoP-5-100, NiMoP-5-130, NiMoP-5-160, and NiMoP-5-180 are approximately 1.6 mg cm -2 , 1.1 mg cm -2 , 1.5 mg cm -2 and 1.2 mg cm -2 .

[0151] The electrochemical performance of NiMoP-5-100 was tested, and the results are as follows Fig. 20 As shown. Among them, Fig. 20 (a) is the CV curve of NiMoP-5-100 at different scan rates; Fig. 20 (b) is the charge and discharge curve of NiMoP-5-100 at different current densities; the oxidation peak values ​​at different scan rates obtained according to the CV curve are shown in Table 5, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 6.

[0152] The electrochemical performance of NiMoP-5-130 was tested, and the results are as follows Fig.21 As shown. Among them, Fig.21 (a) is the CV curve of NiMoP-5-130 at different scan rates; Fig.21 (b) is the charge and discharge curve of NiMoP-5-130 at different current densities; the oxidation peaks at different scan rates obtained according to the CV curves are shown in Table 5, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 6.

[0153] The electrochemical performance of NiMoP-5-160 was tested, and the results are as follows Fig. 22 As shown. Among them, Fig. 22 (a) shows the CV curves of NiMoP-5-160 at different scan rates; Fig. 22 (b) is the charge and discharge curve of NiMoP-5-160 at different current densities; the oxidation peak values ​​at different scan rates obtained according to the CV curve are shown in Table 5, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 6.

[0154] The electrochemical performance of NiMoP-5-180 was tested, and the results are as follows Fig.23 As shown. Among them, Fig.23 (a) shows the CV curves of NiMoP-5-180 at different scan rates; Fig.23 (b) is the charge and discharge curve of NiMoP-5-180 at different current densities; the oxidation peak values ​​at different scan rates obtained according to the CV curve are shown in Table 5, and the specific capacity results at different current densities calculated according to the charge and discharge curves are shown in Table 6.

[0155] Depend on Figures 20-23 As shown in (a), a pair of obvious redox peaks appear in the CV curve, indicating that the electrode material undergoes a redox reaction during the charge transfer process, indicating that the energy storage behavior of the electrode material is pseudocapacitive behavior. It can be observed from the figure that as the scan rate increases, the oxidation peak and reduction peak in the CV curve move toward the potential boundary, which is caused by the resistance and polarization of the electrode itself.

[0156] Depend on Figures 20-23 As shown in (b), the charge and discharge curves of all electrode materials have obvious discharge platforms, which are typical battery-type materials. When the current density increases from 1A / g to 10A / g, the charge and discharge time of the electrode material is significantly shortened. This may be because under high current density conditions, the electrode active material fails to fully participate in the redox reaction, and the low ion diffusion rate cannot meet the rapid redox reaction under high current density, resulting in low utilization of the electrode material. The GCD curve is a symmetrical nonlinear charge and discharge curve, indicating that the electrode has good chemical reversibility.

[0157] Fig.24 1 is a comparison diagram of the electrochemical performance of the electrode materials prepared in Examples 10 to 13 under the same test conditions. Among them, the CV comparison curves of the electrode materials prepared in Examples 10 to 13 at a scan rate of 6 mV / s are as follows: Fig.24 As shown in (a), the charge and discharge comparison curves of the electrode materials prepared in Examples 10 to 13 at a current density of 1 A / g are as follows: Fig.24 As shown in (b).

[0158] Depend on Fig.24 (a) It can be seen that at the same scan rate, the CV integral area of ​​the NiMoP-5-160 electrode material prepared at a hydrothermal temperature of 160°C is the largest, and the peak current is the largest. Fig.24 (b) It can be seen that the discharge time of NiMoP-5-160 is the longest.

[0159] Table 5 Oxidation peak values ​​of NiMoP materials prepared at different temperatures at different scan rates

[0160] 1mV / s 2mV / s 3mV / s 4mV / s 5mV / s 6mV / s 7mV / s 8mV / s 9mV / s 10mV / s NiMoP-5-100 0.486 0.494 0.497 0.500 0.502 0.503 0.504 0.506 0.507 0.509 NiMoP-5-130 0.487 0.492 0.498 0.502 0.506 0.510 0.513 0523 0.527 0.526 NiMoP-5-160 0.499 0.517 0.521 0.534 0.547 0.560 0.552 0.561 0.554 0.558 NiMoP-5-180 0.512 0.521 0.529 0.535 0.540 0.545 0.549 0.553 0.557 0.560

[0161] Table 6 Specific capacity (mAh / g) of NiMoP materials prepared at different temperatures at different current densities

[0162] 1A / g 3A / g 5A / g 7A / g 9A / g 10A / g NiMoP-5-100 39.1 35.8 34.3 33.1 32.0 31.7 NiMoP-5-130 70.6 65.4 63.1 61.3 59.7 59.2 NiMoP-5-160 331.7 293.3 277.2 217.8 210.7 205.3 NiMoP-5-180 229.4 327.8 337.9 316.4 304.5 299.2

[0163] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a NiMoP electrode material, characterized in that: The following steps are involved: A soluble nickel salt, a soluble molybdenum source, a soluble phosphate, a conductive substrate and water are mixed for hydrothermal reaction to obtain a nickel-molybdenum-based phosphate; The nickel-molybdenum-based phosphate is calcined to generate nickel-molybdenum phosphide to obtain the NiMoP electrode material; The ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:1-8; The ratio of the amount of nickel in the soluble nickel salt to the amount of molybdenum in the soluble molybdenum source is 1:1; The temperature of the hydrothermal reaction is 100-180° C., and the time is 3-15 hours.

2. The preparation method according to claim 1, characterized in that: The soluble nickel salt includes one or more of nickel acetate, nickel nitrate and nickel sulfate.

3. The preparation method according to claim 1, characterized in that: The soluble molybdenum source includes one or more of sodium molybdate, ammonium molybdate and molybdic acid.

4. The preparation method according to claim 1, characterized in that: The soluble phosphate includes one or more of sodium hypophosphite, sodium dihydrogen phosphate and potassium dihydrogen phosphate.

5. The preparation method according to claim 1, characterized in that: The ratio of the amount of nickel in the soluble nickel salt to the amount of phosphorus in the soluble phosphate is 1:5; The temperature of the hydrothermal reaction is 160° C. and the time is 12 h.

6. The preparation method according to claim 1, characterized in that: The calcination temperature is 300-600° C. and the calcination time is 1-6 hours.

7. The NiMoP electrode material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The NiMoP is supported on a conductive substrate, and the shape of the NiMoP includes sphere and / or flake.

8. The NiMoP electrode material according to claim 7, characterized in that: The loading amount of NiMoP on the conductive substrate is 1.1-1.8 mg·cm -2 .

9. The NiMoP electrode material according to claim 7, characterized in that: When the NiMoP is spherical, the diameter of the NiMoP is 1 to 2 μm; when the NiMoP is flake-shaped, the length of the NiMoP is 1 to 3 μm; and the thickness is 50 to 200 nm.

10. Use of the NiMoP electrode material according to any one of claims 7 to 9 in a supercapacitor.