High aspect ratio aluminum etching method

Through a two-step plasma etching method, chlorine and boron trichloride are used to generate a passivation layer, and fluorocarbon element polymer gas is added when the etching rate is reduced, which solves the problem of the side of the aluminum etching process in semiconductor devices with high-deep and aspect ratio in semiconductor devices. The problem of corrosion improves the line width stability and product yield of the aluminum metal layer.

CN118943022APending Publication Date: 2024-11-12GTA SEMICON CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410958108.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the metal interconnection line etching process of semiconductor devices, high-deep aspect ratio aluminum etching is prone to side etching in the area near the bottom of the etching groove, causing fluctuations in the line width of the aluminum metal layer and affecting product yield.

Method used

Using a two-step plasma etching method, the first step is to use a mixed gas of chlorine and boron trichloride and nitrogen to etch it to generate an AlxNy passivation layer to protect the aluminum surface; when the etching rate decreases, the fluorine-containing element is added Polymer gas, forming CxHyFz polymer to prevent the reaction of the etching gas with the side wall and reduce side erosion.

Benefits of technology

It effectively reduces the sidewall etching rate, maintains the perpendicularity and accuracy of the aluminum metal layer, avoids the formation of sidewall etching grooves, and improves product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943022A_ABST
    Figure CN118943022A_ABST
Patent Text Reader

Abstract

The invention provides a high aspect ratio aluminum etching method. When an aluminum metal layer is formed through two steps of plasma etching, first-step plasma etching is carried out on an aluminum layer based on a patterned photoresist layer; the etching gas for the first-step plasma etching is mixed gas of chlorine and boron trichloride, and the passivation gas is nitrogen; when the etching rate of the first-step plasma etching is reduced within 25%, carrying out second-step plasma etching on the aluminum layer and the isolation buffer layer; and in the second-step plasma etching, on the premise that the parameter condition of the second-step plasma etching is kept the same as the parameter condition of the first-step plasma etching, polymer gas containing fluorocarbon elements is added in passivation gas, and the ratio of the flow of nitrogen to the flow of the polymer gas containing fluorocarbon elements is 1: (1-2). According to the etching method, side etching of the etching gas on the side wall of the groove can be reduced, formation of a side etching groove is weakened or even avoided, the line width of the aluminum metal interconnection layer formed by high aspect ratio aluminum etching is guaranteed, and the product yield is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor manufacturing, and in particular to a high aspect ratio aluminum etching method. Background Art

[0002] In semiconductor devices, aluminum is the most common interconnect metal layer material. When forming metal interconnects of semiconductor devices, aluminum needs to be etched using etching technology to form metal interconnects. Usually, in order to ensure the line accuracy of the connecting line, a dry etching process is used as a conventional etching method for the aluminum layer, and the aluminum layer is etched using a photoresist as a mask.

[0003] Due to the limitation of photolithography exposure process, the thickness of photoresist with small line width is very limited, which leads to the bottleneck of aspect ratio of aluminum etching process. For example, the aspect ratio of 0.15μm BCD aluminum etching process in common process platform is about 1.7:1, and the aspect ratio of MCU aluminum etching process is about 1.9:1. In addition, the loading effect of high aspect ratio etching due to the influence of pattern density is more serious. Fig. 9 As shown, during the etching process of aluminum with a high aspect ratio, side etching is likely to occur near the bottom of the etching groove 20, forming a Fig. 9 The side etching groove 21 in the aluminum metal layer 22 causes the line width of the aluminum metal layer 22 to fluctuate, mainly narrowing the line width of the aluminum metal layer 22, such as Fig. 9 The aluminum metal layer 22 at A in the middle has side etching on the bottom areas on both sides, and side etching grooves 21 are formed on both sides, which makes the line width of the aluminum metal layer 22 here narrower. In severe cases, the aluminum metal layer 22 may collapse, affecting the product yield. Summary of the invention

[0004] In view of the shortcomings of the prior art described above, the purpose of the present invention is to provide a high aspect ratio aluminum etching method, which is used to solve the problem that when high aspect ratio aluminum is etched to form an interconnection metal layer in the back-end metal interconnection process of a semiconductor device in the prior art, side etching is easily caused in the area near the bottom of the etched groove, affecting the line width of the aluminum metal interconnection layer, resulting in the morphology of the aluminum metal interconnection layer not meeting the device requirements, thereby reducing the product yield.

[0005] To achieve the above objectives and other related objectives, the present invention provides a high aspect ratio aluminum etching method, the etching method comprising:

[0006] Providing a semiconductor substrate, on which an insulating dielectric layer is formed;

[0007] forming an isolation buffer layer and an aluminum layer in sequence on the insulating dielectric layer;

[0008] forming a patterned photoresist layer on the aluminum layer;

[0009] The aluminum layer is subjected to a first step of plasma etching based on the patterned photoresist layer; wherein the etching gas for the first step of plasma etching is a mixed gas of chlorine and boron trichloride, and the passivation gas is nitrogen;

[0010] When the etching rate of the first plasma etching is reduced to less than 25%, the aluminum layer and the isolation buffer layer are subjected to a second plasma etching based on the patterned photoresist layer; wherein, the second plasma etching is performed while maintaining the same parameters as the first plasma etching, and a polymer gas containing carbon fluorine elements is added to the passivation gas, and the flow rate of the nitrogen gas:the flow rate of the polymer gas containing carbon fluorine elements=1:(1-2);

[0011] The patterned photoresist layer is removed.

[0012] Optionally, when the etching rate of the first step of plasma etching is reduced to within 15% to 25%, the second step of plasma etching is performed.

[0013] Optionally, the isolation buffer layer is a titanium layer, and the aluminum layer is a copper-doped aluminum layer.

[0014] Furthermore, the thickness of the isolation buffer layer is The thickness of the aluminum layer is The thickness of the patterned photoresist layer is

[0015] Optionally, the method for forming the patterned photoresist layer includes: first forming a photoresist layer on the aluminum layer; and then exposing and developing the photoresist layer to obtain the patterned photoresist.

[0016] Optionally, after forming the aluminum layer and before forming the patterned photoresist layer, a step of forming a bottom anti-reflection layer on the aluminum layer is also included; and the first step of plasma etching also includes etching the bottom anti-reflection layer.

[0017] Optionally, the flow rate of the chlorine gas in the etching gas: the flow rate of the boron trichloride = (2-3):1.

[0018] Furthermore, the chamber pressure of the etching chamber of the first step plasma etching and the second step plasma etching is 8mTorr-12mTorr, the ionization power of the plasma is 600W-800W, and the bias power of the plasma is 40W-60W.

[0019] Furthermore, the flow rate of the nitrogen gas is 5 sccm to 15 sccm.

[0020] Optionally, the polymer gas containing carbon fluorine elements is CHF3 or CF4 or CH2F2.

[0021] As described above, the high aspect ratio aluminum etching method of the present invention is completed by two-step plasma etching when etching to form an aluminum metal layer. In the first step of plasma etching, the etching gas uses a mixed gas of chlorine and boron trichloride combined with a nitrogen passivation gas. The nitrogen can react with aluminum to generate Al x N y The passivation layer, the Al x N y The passivation layer can protect the aluminum surface from being over-etched, which helps to improve the selectivity of aluminum etching, so that the etching process can more accurately remove the unnecessary aluminum material (i.e., the aluminum material in the vertical direction) while retaining the required aluminum structure. x N y The passivation layer is formed on the sidewalls of the trench, which can reduce the etching rate of the sidewalls, thereby maintaining the verticality and accuracy of the structure, but Al x N y The passivation layer needs to react with aluminum to form, which is passive. During the etching process, it will react with the etching gas to generate aluminum chloride gas. Therefore, the nitrogen passivation gas has limited protection for the side wall during aluminum etching. When the etching rate decreases, the etching time of the side wall is prolonged. x N y The protective effect of the passivation layer on the side wall is weakened. The study found that when the etching rate of the first step of plasma etching is reduced to less than 25%, the improvement of the side wall side etching is most effective when entering the second step of plasma etching. The second step of plasma etching, while maintaining the same parameters as the first step of plasma etching, adds a polymer gas containing carbon fluorine elements to the passivation gas, and makes the flow rate of nitrogen and the flow rate of the polymer gas containing carbon fluorine elements in the parameter range of 1: (1-2). The C x H y F z The polymer has excellent adhesion. After entering the etched groove, it does not need to react with aluminum. It can directly adhere to the side wall of the groove without reacting with aluminum. It can effectively block the reaction between the etching gas and the side wall. Due to the directional selection of plasma etching, the C x H y F z Polymer bombardment removal achieves downward etching of aluminum material, while the bombardment effect of plasma on the trench sidewall is very weak, thereby reducing the side etching of the trench sidewall by the etching gas, weakening or even avoiding the formation of side etching grooves, ensuring the line width of the aluminum metal interconnect layer formed by high aspect ratio aluminum etching, and improving product yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figures 1 to 7Shown is a schematic diagram of the cross-sectional structure of each step in the high aspect ratio aluminum etching method of the present invention.

[0023] Figure 8 Shown is a SEM image of an aluminum metal layer prepared by the high aspect ratio aluminum etching method of the present invention.

[0024] Fig. 9 An SEM image of an aluminum metal layer is shown as an example in the prior art.

[0025] Description of Figure Numbers

[0026] 10 Semiconductor substrate

[0027] 11 Insulation dielectric layer

[0028] 12 Isolation buffer layer

[0029] 13 Aluminum layer

[0030] 14 Patterned photoresist layer

[0031] 140 Photoresist layer

[0032] 15 First Groove

[0033] 16 Second groove

[0034] 17 Bottom anti-reflection layer

[0035] 18 Aluminum metal layer

[0036] 20 Etching groove

[0037] 21 Side Etching Groove

[0038] 22 Aluminum metal layer DETAILED DESCRIPTION

[0039] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0040] See also Figures 1 to 8 It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0041] As described in the background technology, Fig. 9 As shown in FIG. 1 , during the etching process of aluminum with a high aspect ratio, side etching is likely to occur near the bottom of the etching groove 20, forming a Fig. 9 The side etching groove 21 in the aluminum metal layer 22 causes the line width of the aluminum metal layer 22 to fluctuate, which is mainly manifested as the narrowing of the line width of the aluminum metal layer 22. The inventor has conducted in-depth research on this issue and believes that in the process of etching aluminum with a high aspect ratio using a plasma dry etching process, the energy of the plasma will be relatively reduced at a deeper depth, and the corresponding vertical etching rate will also be reduced, so that a longer etching time is required at a deeper depth, resulting in a longer etching time for the side walls of the grooves at a deeper depth relative to the side walls of the grooves at a shallower depth. In addition, the plasma dry etching process is more inclined to chemical etching for metal etching, that is, the physical bombardment etching of the plasma is weaker, so that a longer etching time will cause side etching on the side walls of the bottom area of ​​the deep groove, and the greater the aspect ratio of the groove, the more obvious this phenomenon is.

[0042] Based on the above cognition and analysis, the inventors found that the plasma dry etching process will inevitably produce a relatively weaker energy of the plasma as it etches thicker metal materials and needs to form an etching groove with a high aspect ratio. This is because the longer the travel of the reactant plasma is, the lower the energy is. In addition, the byproducts produced by etching will collide with the reactant plasma to reduce the energy of the reactant plasma. Therefore, the longer the etching time is required, the longer the etching time is. At this time, it can be considered that when the etching rate decreases, that is, when a longer etching time is required, the etching rate of the side wall can be reduced, thereby reducing the side etching of the groove side wall. From this perspective, this embodiment provides a high aspect ratio aluminum etching method, and the etching method includes:

[0043] S1. providing a semiconductor substrate, on which an insulating dielectric layer is formed;

[0044] S2, sequentially forming an isolation buffer layer and an aluminum layer on the insulating dielectric layer;

[0045] S3, forming a patterned photoresist layer on the aluminum layer;

[0046] S4, performing a first plasma etching on the aluminum layer based on the patterned photoresist layer; wherein the etching gas for the first plasma etching is a mixed gas of chlorine and boron trichloride, and the passivation gas is nitrogen;

[0047] S5. When the etching rate of the first plasma etching is reduced to less than 25%, the aluminum layer and the isolation buffer layer are subjected to a second plasma etching based on the patterned photoresist layer; wherein, the second plasma etching is performed while maintaining the same parameters as the first plasma etching, and a polymer gas containing carbon fluorine elements is added to the passivation gas, and the flow rate of the nitrogen gas:the flow rate of the polymer gas containing carbon fluorine elements=1:(1-2);

[0048] S6. removing the patterned photoresist layer.

[0049] The high aspect ratio aluminum etching method of this embodiment is completed by two-step plasma etching when etching to form an aluminum metal layer. In the first step of plasma etching, the etching gas uses a mixed gas of chlorine and boron trichloride combined with a nitrogen passivation gas. Nitrogen can react with aluminum to generate Al x N y The passivation layer, the Al x N y The passivation layer can protect the aluminum surface from being over-etched, which helps to improve the selectivity of aluminum etching, so that the etching process can more accurately remove the unnecessary aluminum material (i.e., the aluminum material in the vertical direction) while retaining the required aluminum structure. x N y The passivation layer is formed on the sidewalls of the trench, which can reduce the etching rate of the sidewalls, thereby maintaining the verticality and accuracy of the structure, but Al x N y The passivation layer needs to react with aluminum to form, which is passive. During the etching process, it will react with the etching gas to generate aluminum chloride gas. Therefore, the nitrogen passivation gas has limited protection for the side wall during aluminum etching. When the etching rate decreases, the etching time of the side wall is prolonged. x N y The protective effect of the passivation layer on the side wall is weakened. The study found that when the etching rate of the first step of plasma etching is reduced to less than 25%, the improvement of the side wall side etching is most effective when entering the second step of plasma etching. The second step of plasma etching, while maintaining the same parameters as the first step of plasma etching, adds a polymer gas containing carbon fluorine elements to the passivation gas, and makes the flow rate of nitrogen and the flow rate of the polymer gas containing carbon fluorine elements in the parameter range of 1: (1-2). The C x H y F z The polymer has excellent adhesion. After entering the etched groove, it does not need to react with aluminum. It can directly adhere to the side wall of the groove without reacting with aluminum. It can effectively block the reaction between the etching gas and the side wall. Due to the directional selection of plasma etching, the C x Hy F z Polymer bombardment removal achieves downward etching of aluminum material, while the bombardment effect of plasma on the trench sidewall is very weak, thereby reducing the side etching of the trench sidewall by the etching gas, weakening or even avoiding the formation of side etching grooves, ensuring the line width of the aluminum metal interconnect layer formed by high aspect ratio aluminum etching, and improving product yield.

[0050] The high aspect ratio aluminum etching method of this embodiment is described in detail below with reference to the specific drawings.

[0051] like Figure 1 As shown, step S1 is first performed to provide a semiconductor substrate 10 , on which an insulating dielectric layer 11 is formed.

[0052] The semiconductor substrate 10 has completed the front-end process of the semiconductor device to form the circuit structure of the chip. The insulating dielectric layer 11 formed on the semiconductor substrate 10 is used to insulate and protect the circuit structure formed by the front-end process and expose the pads for circuit interconnection. Subsequently, a back-end metal interconnection structure is formed on the semiconductor substrate 10, wherein the metal interconnection layer and the metal interconnection pillar are protected. This embodiment mainly proposes an etching method for the aluminum metal interconnection layer in the back-end metal interconnection structure.

[0053] As an example, the material selection of the semiconductor substrate 10 is based on the needs of the semiconductor device, and any suitable semiconductor material can be selected, such as: a single layer structure of Si, Ge, SiGe, SiC, SiGeC, InAs, GaAs, InP, InGaAs or other III / V compound semiconductors; it can also be a multi-layer stacked structure composed of these semiconductor materials; it can also be silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI), etc. The insulating dielectric layer 11 selects any suitable dielectric protection material layer, and the commonly used one in the industry is a silicon dioxide insulating dielectric layer.

[0054] like Figure 2 As shown, step S2 is then performed to sequentially form an isolation buffer layer 12 and an aluminum layer 13 on the insulating dielectric layer 11. It should be noted that this embodiment is mainly about the preparation of the back-end metal interconnect structure, so the semiconductor substrate 10 is omitted in the subsequent drawings for ease of understanding.

[0055] Since aluminum and the semiconductor substrate 10 may diffuse and penetrate each other, an isolation buffer layer 12 is provided between the insulating dielectric layer 11 and the aluminum layer 13 as a barrier layer therebetween. As an example, the isolation buffer layer 12 is a titanium layer, or a stack of a titanium layer and a titanium nitride layer.

[0056] When pure aluminum is used as the metal interconnect layer, electromigration may occur when current flows through the aluminum interconnect line. Therefore, the aluminum layer 13 may preferably be a copper-doped aluminum layer. Since copper atoms are heavier than aluminum atoms, the movement of aluminum single crystal particles may be effectively suppressed, thereby improving the electromigration problem.

[0057] As an example, the isolation buffer layer 12 may be formed by CVD or PVD; and the aluminum layer 13 may be formed by PVD.

[0058] As a specific example, when the isolation buffer layer 12 is selected as a titanium layer and the aluminum layer 13 is selected as a copper-doped aluminum layer, the thickness of the isolation buffer layer 12 is selected as The thickness of the aluminum layer 13 is selected to be

[0059] like Figure 5 As shown, step S3 is then performed to form a patterned photoresist layer 14 on the aluminum layer 13 .

[0060] like Figure 3 As shown, as an example, after forming the aluminum layer 13 and before forming the patterned photoresist layer 14, a step of forming a bottom anti-reflection layer 17 on the aluminum layer 13 is also included. The bottom anti-reflection layer 17 can absorb the reflected light during photolithography to prevent the pattern size of the photoresist layer from deviating. In this embodiment, the bottom anti-reflection layer 17 can be selected as a dielectric anti-reflection layer, and the material can be silicon nitride or silicon oxynitride; when the material of the bottom anti-reflection layer 17 is selected as silicon oxynitride, the thickness is generally selected to be

[0061] like Figures 3 to 5 As shown, as a specific example, the method of forming the patterned photoresist layer 14 includes: Figure 4 As shown, a photoresist layer 140 is first formed on the aluminum layer 13, as shown in FIG. Figure 3 As shown in FIG. 1 , when the bottom anti-reflection layer 17 is formed on the aluminum layer 13, the photoresist layer 140 is as shown in FIG. Figure 4 As shown, it is coated on the surface of the bottom anti-reflection layer 17; Figure 5 As shown, the photoresist layer 140 is then exposed and developed to obtain the patterned photoresist layer 14. Based on the effect of the bottom anti-reflection layer 17, the reflected light can be absorbed during the exposure process, so that the patterned photoresist layer 14 can obtain satisfactory conformality.

[0062] As an example, when the isolation buffer layer 12 is selected as a titanium layer, the aluminum layer 13 is selected as a copper-doped aluminum layer, and the thickness of the isolation buffer layer 12 is selected as The thickness of the aluminum layer 13 is selected to be When the thickness of the photoresist layer 140 is selected to be

[0063] like Figure 6 As shown, step S4 is then performed to perform the first plasma etching on the aluminum layer 13 based on the patterned photoresist layer 14; wherein the etching gas of the first plasma etching is a mixed gas of chlorine and boron trichloride, and the passivation gas is nitrogen, to form a first groove 15.

[0064] like Figure 6 As shown, as an example, when the bottom anti-reflection layer 17 is formed on the aluminum layer 13 , the first plasma etching of this step also includes etching the bottom anti-reflection layer 17 .

[0065] In the first plasma etching process of this step, the passivation gas nitrogen will react with aluminum to form Al x N y The passivation layer is an amorphous structure. The etching gas will react with the Al x N y The passivation layer reacts and also reacts with the aluminum layer to etch the aluminum layer. On the other hand, the passivation gas will continue to react with the aluminum layer to generate an amorphous structure of Al x N y The passivation layer is continuously circulated in this way to inhibit the over-etching of aluminum by the etching gas, realize the vertical etching of the aluminum layer and ensure the smoothness and uniformity of the side wall.

[0066] As an example, the flow rate of the chlorine gas in the etching gas: the flow rate of the boron trichloride = (2-3): 1. On this basis, preferably, during the first step of plasma etching, the chamber pressure of the etching chamber is 8mTorr-12mTorr, the ionization power of the plasma is 600W-800W, and the bias power of the plasma is 40W-60W. Furthermore, the flow rate of the nitrogen gas is 5sccm-15sccm.

[0067] The end of the first step of plasma etching is adjusted based on the reduction of its etching rate. It has been found that when the etching rate of the first step of plasma etching is reduced within 25%, the second step of plasma etching can be entered, and it is preferably selected when the etching rate of the first step of plasma etching is reduced within 15% to 25% to carry out the second step of plasma etching.

[0068] like Figure 7As shown, step S5 is performed, when the etching rate of the first plasma etching is reduced to within 25%, the aluminum layer 13 and the isolation buffer layer 12 are subjected to a second plasma etching based on the patterned photoresist layer 14; wherein, the second plasma etching, while maintaining the same parameters as the first plasma etching, adds a polymer gas containing carbon fluorine elements to the passivation gas (that is, on the basis of the first plasma etching, the introduction of a polymer gas containing carbon fluorine elements is increased in the etching chamber), and the flow rate of the nitrogen gas: the flow rate of the polymer gas containing carbon fluorine elements = 1: (1~2), to form a second groove 16, and an aluminum metal layer 18 is formed between two adjacent second grooves 16.

[0069] In the second step of plasma etching, the C x H y F z The polymer has excellent adhesion. After entering the etched groove, it does not need to react with aluminum. It can directly adhere to the side wall of the groove without reacting with aluminum. It can effectively block the reaction between the etching gas and the side wall. Due to the directional selection of plasma etching, the C x H y F z Polymer bombardment removal achieves downward etching of aluminum material, while the bombardment effect of plasma on the trench sidewall is very weak, thereby reducing the side etching of the trench sidewall by the etching gas, weakening or even avoiding the formation of side etching grooves, ensuring the line width of the aluminum metal interconnect layer formed by high aspect ratio aluminum etching, and improving product yield.

[0070] As an example, the polymer gas containing carbon fluorine elements can be selected as CHF3 or CF4 or CH2F2. In this embodiment, CHF3 is preferably selected.

[0071] like Figure 8 , which is a SEM image of an aluminum metal layer prepared by the high aspect ratio aluminum etching method of this embodiment, the parameters used are: the isolation buffer layer 12 is selected as a titanium layer, the aluminum layer 13 is selected as a copper-doped aluminum layer, and the thickness of the isolation buffer layer 12 is selected to be approximately The thickness of the aluminum layer 13 is selected to be approximately The material of the bottom anti-reflection layer 17 is silicon oxynitride, and the thickness of the bottom anti-reflection layer 17 is about The thickness of the patterned photoresist layer 14 is selected to be approximately The flow rate of the chlorine gas in the etching gas is about 2:1 to the flow rate of the boron trichloride. The chamber pressure of the first plasma etching and the second plasma etching is about 10 mTorr, the ionization power of the plasma is 600W to 800W, the bias power of the plasma is 40W to 60W, and the flow rate of the nitrogen is 5 sccm to 15 sccm. The depth-to-width ratio of the second trench 16 formed after etching can reach 4:1, and compared with Figure 8 and Fig. 9 It can be clearly seen Figure 8 The smoothness of the side wall of the aluminum metal layer 18 formed in the process is greatly improved, and there is basically no side erosion.

[0072] like Figure 7 As shown, step S6 is finally performed to remove the patterned photoresist layer 14 .

[0073] The patterned photoresist layer 14 may be removed by using an existing conventional photoresist removal method.

[0074] In summary, the present invention provides a high aspect ratio aluminum etching method, which is completed by two-step plasma etching when etching to form an aluminum metal layer. In the first step of plasma etching, the etching gas uses a mixed gas of chlorine and boron trichloride combined with a nitrogen passivation gas, and the nitrogen can react with aluminum to generate Al x N y The passivation layer, the Al x N y The passivation layer can protect the aluminum surface from being over-etched, which helps to improve the selectivity of aluminum etching, so that the etching process can more accurately remove the unnecessary aluminum material (i.e., the aluminum material in the vertical direction) while retaining the required aluminum structure. x N y The passivation layer is formed on the sidewalls of the trench, which can reduce the etching rate of the sidewalls, thereby maintaining the verticality and accuracy of the structure, but Al x N y The passivation layer needs to react with aluminum to form, which is passive. During the etching process, it will react with the etching gas to generate aluminum chloride gas. Therefore, the nitrogen passivation gas has limited protection for the side wall during aluminum etching. When the etching rate decreases, the etching time of the side wall is prolonged. x N y The protective effect of the passivation layer on the side wall is weakened. The study found that when the etching rate of the first step of plasma etching is reduced to less than 25%, the improvement of the side wall side etching is most effective when entering the second step of plasma etching. The second step of plasma etching, while maintaining the same parameters as the first step of plasma etching, adds a polymer gas containing carbon fluorine elements to the passivation gas, and makes the flow rate of nitrogen and the flow rate of the polymer gas containing carbon fluorine elements in the parameter range of 1: (1-2). The Cx H y F z The polymer has excellent adhesion. After entering the etched groove, it does not need to react with aluminum. It can directly adhere to the side wall of the groove without reacting with aluminum. It can effectively block the reaction between the etching gas and the side wall. Due to the directional selection of plasma etching, the C x H y F z The polymer bombardment removal realizes the downward etching of aluminum material, while the bombardment effect of plasma on the side wall of the groove is very weak, thereby reducing the side etching of the groove side wall by the etching gas, weakening or even avoiding the formation of the side etching groove, ensuring the line width of the aluminum metal interconnection layer formed by the high aspect ratio aluminum etching, and improving the product yield. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.

[0075] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A high aspect ratio aluminum etching method, characterized in that: The etching method comprises: Providing a semiconductor substrate, on which an insulating dielectric layer is formed; forming an isolation buffer layer and an aluminum layer in sequence on the insulating dielectric layer; forming a patterned photoresist layer on the aluminum layer; Based on the patterned photoresist layer, the aluminum layer is subjected to a first plasma etching; wherein the etching gas of the first plasma etching is a mixed gas of chlorine and boron trichloride, and the passivation gas is nitrogen; When the etching rate of the first plasma etching is reduced to within 25%, the aluminum layer and the isolation buffer layer are subjected to a second plasma etching based on the patterned photoresist layer; wherein, the second plasma etching is performed while maintaining the same parameters as the first plasma etching, and a polymer gas containing carbon fluorine elements is added to the passivation gas, and the flow rate of the nitrogen gas: the flow rate of the polymer gas containing carbon fluorine elements = 1: (1~2); The patterned photoresist layer is removed.

2. The high aspect ratio aluminum etching method according to claim 1, characterized in that: When the etching rate of the first step plasma etching is reduced to within 15% to 25%, the second step plasma etching is performed.

3. The high aspect ratio aluminum etching method according to claim 1, characterized in that: The isolation buffer layer is a titanium layer, and the aluminum layer is a copper-doped aluminum layer.

4. The high aspect ratio aluminum etching method according to claim 3, characterized in that: The thickness of the isolation buffer layer is The thickness of the aluminum layer is The thickness of the patterned photoresist layer is 5. The high aspect ratio aluminum etching method according to claim 1, characterized in that: The method for forming the patterned photoresist layer comprises: first forming a photoresist layer on the aluminum layer; then exposing and developing the photoresist layer to obtain the patterned photoresist layer.

6. The high aspect ratio aluminum etching method according to claim 1, characterized in that: After forming the aluminum layer and before forming the patterned photoresist layer, a step of forming a bottom anti-reflection layer on the aluminum layer is also included; and the first step of plasma etching also includes etching the bottom anti-reflection layer.

7. The high aspect ratio aluminum etching method according to claim 1, characterized in that: The flow rate of the chlorine gas in the etching gas: the flow rate of the boron trichloride = (2-3):

1.

8. The high aspect ratio aluminum etching method according to claim 7, characterized in that: The chamber pressure of the etching chamber of the first step plasma etching and the second step plasma etching is 8mTorr-12mTorr, the ionization power of the plasma is 600W-800W, and the bias power of the plasma is 40W-60W.

9. The high aspect ratio aluminum etching method according to claim 8, characterized in that: The flow rate of the nitrogen gas is 5 sccm to 15 sccm.

10. The high aspect ratio aluminum etching method according to claim 1, characterized in that: The polymer gas containing carbon fluorine elements is CHF3 or CF4 or CH2F2.

Citation Information

Cited By

  • Etching method and semiconductor process equipment

    CN120769574A