Selective passivation contact structure, solar cell and manufacturing method thereof
By forming a selective passivation contact structure on the silicon wafer of solar cells, the passivation contact structure of ultra-thin tunneling oxide layer and highly doped polysilicon layer is solved, the light-shading problem of TOPCon cell is improved, and the conversion efficiency is avoided. Silicon-based loss is achieved, and higher photoelectric conversion efficiency is achieved.
Patent Information
- Application Number
- CN202410858815.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-12
AI Technical Summary
TOPCon solar cells have light shading problems caused by the increase in metal gate lines in order to improve the filling factor (FF), which leads to a reduction in cell conversion efficiency. The prior art relies on laser selective emitter technology, and there is a risk of silicon-based loss.
Using a selective passivation contact structure, an ultra-thin tunneling oxide layer and a highly doped polysilicon layer are deposited on the front and back of the silicon wafer respectively to form a passivation contact structure, reducing the metal contact recombination current, and forming a blunt part on the light-receiving surface. The layer reduces parasitic absorption and improves the carrier absorption capacity.
It is achieved to improve the conversion efficiency of solar cells without increasing the number of gate lines, avoid the silicon-based losses caused by laser selective emitters, expand the technical matching space, and improve the photoelectric conversion efficiency of the cell.
Smart Images

Figure HDA0004918876270000011
Abstract
Description
Technical Field
[0001] The present application relates to the field of solar cells, and in particular to a selective passivation contact structure and a solar cell and a method for manufacturing the same. Background Art
[0002] The silicon oxide at the interface between the Poly-Si and Si substrate of the TOPCon passivated contact cell plays a very critical role in passivation. Silicon oxide reduces the interface state density between the Si substrate and the Poly-Si through its chemical passivation. The majority carrier concentration is much higher than the minority carrier concentration, which reduces the probability of electron-hole recombination while increasing the resistivity to form selective contact for the majority carriers.
[0003] Tunnel oxide passivation contact (TOPCon) uses an ultra-thin tunnel SiO2 layer to cover doped polysilicon, providing passivation and carrier selectivity respectively. Con-based cells have an additional benefit of being compatible with traditional fire-resistant screen-printed metallization, making them compatible with existing solar cell production lines. Although having full-area polysilicon contacts on both sides of the solar cell can produce VOCs up to 728mV, the thick polysilicon layer of the TOPCon cell causes significant current losses due to parasitic absorption, but on the other hand, the thin polysilicon layer will cause the paste to burn through the tunneling layer and directly contact the silicon substrate during metal sintering, affecting the ohmic contact, resulting in higher J0 (current density), limiting the cell's higher efficiency. Summary of the invention
[0004] The biggest influence on FF (fill factor) of existing TOPCon battery technology is the square resistance loss of p+-poly. The most direct and commonly used technology to improve FF is dense grid, that is, increasing the number of metal grid lines, so that a larger contact area can also achieve a higher FF. However, continuing to increase the number of metal grid lines will increase the shading of the battery cell surface, resulting in a reduction in the light-receiving area and thus short-circuit current loss, which will reduce the conversion efficiency of the battery cell.
[0005] In order to solve the problems existing in the prior art, the present application provides a selective passivation contact structure and a solar cell and a method for manufacturing the same.
[0006] Passivation media are usually non-conductive, so there is a contradiction between effective passivation and current extraction. The solution is to use amorphous silicon as the passivation layer, amorphous silicon heterojunction passivation structure (HIT), or use an ultra-thin oxide layer as the passivation layer, a tunneling oxide layer passivated contact structure (PolyPassivated). An ultra-thin tunneling oxide layer and a highly doped polysilicon thin layer are prepared on the back of the battery. The two together form a passivation contact structure, which provides good surface passivation for the back of the silicon wafer. The ultra-thin oxide layer allows majority electrons to tunnel into the polysilicon layer, while blocking the recombination of minority holes, thereby realizing the lateral transmission of electrons in the polysilicon layer and being collected by the metal, greatly reducing the metal contact recombination current and improving the open circuit voltage and short circuit current of the battery.
[0007] Note: In this application, after the substrate is made into a solar cell, the side exposed to sunlight is called the front side, and the other side is called the back side.
[0008] The specific technical solutions of this application are as follows:
[0009] 1. A solar cell with a selective passivation contact structure, wherein the solar cell comprises a substrate, a second passivation layer is arranged on the substrate, and the second passivation layer is arranged on the front side of the substrate;
[0010] Preferably, a first passivation layer is arranged on a side of the substrate facing away from the second passivation layer.
[0011] 2. According to the solar cell described in item 1, the second passivation layer covers a local position of the substrate. Preferably, the second passivation layer covers a local position of the substrate where current or voltage exists. Further preferably, a front grid line is arranged on the substrate, and the second passivation layer is arranged between the front grid line and the substrate.
[0012] 3. According to the solar cell described in item 1 or 2, the second passivation layer includes a tunneling layer; preferably, the second passivation layer also includes a doping layer; further preferably, the second passivation layer includes a tunneling layer and a doping layer stacked in sequence in a front direction.
[0013] 4. According to the solar cell described in any one of items 1 to 3, the first passivation layer includes a tunneling layer. Preferably, the first passivation layer also includes a doping layer. Further preferably, the first passivation layer includes a tunneling layer and a doping layer stacked in sequence in a direction toward the back side.
[0014] 5. According to the solar cell described in any one of items 1 to 4, the doping layers of the first passivation layer and the second passivation layer are doping layers with different dopings; preferably, the doping layer of the first passivation layer is a boron-doped doping layer, and the doping layer of the second passivation layer is a phosphorus-doped doping layer, and further preferably, the doping layer of the first passivation layer is a boron-doped polycrystalline silicon layer, and the doping layer of the second passivation layer is a phosphorus-doped polycrystalline silicon layer.
[0015] 6. The solar cell according to any one of items 1 to 5, wherein a first anti-reflection layer is disposed on the substrate, and the anti-reflection layer is used to improve the utilization of sunlight;
[0016] Preferably, a second anti-reflection layer is provided on the side of the substrate facing away from the first anti-reflection layer;
[0017] Further preferably, the first anti-reflection layer is arranged on a side of the first passivation layer away from the substrate; and the second anti-reflection layer is arranged on a side of the second passivation layer away from the substrate.
[0018] 7. The solar cell according to any one of items 1 to 6, wherein the first anti-reflection layer comprises an aluminum oxide layer, and the second anti-reflection layer comprises an aluminum oxide layer;
[0019] Preferably, the first anti-reflection layer comprises a silicon nitride anti-reflection film, and the second anti-reflection layer comprises a laminated anti-reflection film;
[0020] Further preferably, the first anti-reflection layer comprises a silicon nitride anti-reflection film and an aluminum oxide layer, and the second anti-reflection layer comprises a laminated anti-reflection film and an aluminum oxide layer;
[0021] Further preferably, the first anti-reflection layer is arranged on the back side of the substrate, and the second anti-reflection layer is arranged on the front side of the substrate.
[0022] 8. The solar cell according to any one of items 1 to 7, wherein a back grid line is arranged on the substrate, and the back grid line and the first passivation layer are located on the same side, preferably, the first passivation layer is located between the substrate and the back grid line.
[0023] 9. A method for manufacturing a selectively passivated contact structure, wherein:
[0024] Polish the silicon wafer on both sides.
[0025] Make the back passivation layer and the front passivation layer on the silicon wafer.
[0026] A mask layer is made locally on the front side of the silicon wafer.
[0027] Clean the mask layer on the front side of the silicon wafer and the passivation layer on the front side where the mask layer is not generated.
[0028] A selectively passivated contact structure is obtained;
[0029] When the mask layer is locally formed on the front side, the mask layer is formed at the position of the preset electrode.
[0030] 10. According to the method described in item 9, the mask layer is a silicon oxide mask layer.
[0031] 11. According to the method described in item 9, when forming the mask layer, the mask layer is formed by a laser method.
[0032] 12. According to the method described in item 9, when manufacturing the back passivation layer and the front passivation layer, the back passivation layer is manufactured first and then the front passivation layer is manufactured.
[0033] 13. According to the method described in item 9, when manufacturing the back passivation layer and the front passivation layer, LPCVD method and / or PECVD method are used for manufacturing.
[0034] 14. According to the method described in item 13, when the PECVD method is used to form the back passivation layer, a tunneling oxide layer and a polysilicon layer are deposited on the back side of the silicon wafer to form a back passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0035] 15. According to the method described in item 14, the polysilicon layer deposited on the back side of the silicon wafer is a boron-doped polysilicon layer.
[0036] 16. According to the method described in item 14, the thickness of the tunneling oxide layer deposited on the back side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunneling oxide layer is 1.5 to 2.0 nm.
[0037] 17. According to the method described in item 14, the thickness of the polysilicon layer deposited on the back side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0038] 18. According to the method described in item 14, after the back passivation layer is formed by PECVD, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0039] 19. According to the method described in item 13, when the front passivation layer is prepared by the PECVD method, a tunneling layer and a polysilicon layer are deposited on the front side of the silicon wafer to form a front passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0040] 20. According to the method described in item 19, the polysilicon layer deposited on the front side of the silicon wafer is a phosphorus-doped polysilicon layer.
[0041] 21. According to the method described in item 19, the thickness of the tunneling oxide layer deposited on the front side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunneling oxide layer is 1.5 to 2.0 nm.
[0042] 22. According to the method described in item 19, the thickness of the polysilicon layer deposited on the front side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0043] 23. According to the method described in item 13, when the LPCVD method is used to form the back passivation layer and the front passivation layer, a tunneling oxide layer and a polysilicon layer are simultaneously deposited on the back and front sides of the silicon wafer to form the back passivation layer and the front passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0044] 24. According to the method described in item 23, the thickness of the tunneling oxide layer deposited on the back side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunneling oxide layer is 1.5 to 2.0 nm.
[0045] 25. According to the method described in item 23, the thickness of the polysilicon layer deposited on the back side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0046] 26. According to the method described in item 23, after a polysilicon layer is deposited on a silicon wafer, boron or phosphorus is doped into the polysilicon layer to form a doped polysilicon layer.
[0047] 27. According to the method described in item 23, after the back passivation layer is formed by LPCVD, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0048] 28. According to the method described in item 13, after the back passivation layer is produced by LPCVD, phosphorus is diffused on the front side of the silicon wafer to form a front passivation layer.
[0049] 29. A method for selectively passivating a contact structure of a solar cell, wherein:
[0050] Polish the silicon wafer on both sides.
[0051] Make the back passivation layer and the front passivation layer on the silicon wafer.
[0052] A mask layer is made locally on the front side of the silicon wafer.
[0053] Clean the mask layer on the front side of the silicon wafer and the passivation layer on the front side where the mask layer is not generated.
[0054] Depositing an anti-reflection layer on the silicon wafer,
[0055] Making gate lines on silicon wafers,
[0056] Inject light into silicon wafers and / or sinter them to obtain solar cells;
[0057] When the mask layer is locally formed on the front surface, the mask layer is formed at the position of the preset gate line.
[0058] 30. According to the method described in item 29, the mask layer is a silicon oxide mask layer.
[0059] 31. According to the method described in Item 29, when manufacturing the mask layer, a laser method is used to manufacture the mask layer.
[0060] 32. According to the method described in item 29, when manufacturing the back passivation layer and the front passivation layer, the back passivation layer is manufactured first and then the front passivation layer is manufactured.
[0061] 33. According to the method described in item 29, when manufacturing the back passivation layer and the front passivation layer, LPCVD method and / or PECVD method are used for manufacturing.
[0062] 34. According to the method described in item 33, when the PECVD method is used to form the back passivation layer, a tunneling oxide layer and a polysilicon layer are deposited on the back side of the silicon wafer to form a back passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0063] 35. According to the method described in item 34, the polysilicon layer deposited on the back side of the silicon wafer is a boron-doped polysilicon layer.
[0064] 36. According to the method described in item 34, the thickness of the tunneling oxide layer deposited on the back side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunneling oxide layer is 1.5 to 2.0 nm.
[0065] 37. According to the method described in item 34, the thickness of the polysilicon layer deposited on the back side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0066] 38. According to the method described in item 34, after the back passivation layer is formed by PECVD, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0067] 39. According to the method described in item 33, when the front passivation layer is produced by the PECVD method, a tunneling layer and a polysilicon layer are deposited on the front side of the silicon wafer to form a front passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0068] 40. According to the method described in item 39, the polysilicon layer deposited on the front side of the silicon wafer is a phosphorus-doped polysilicon layer.
[0069] 41. According to the method described in item 39, the thickness of the tunneling oxide layer deposited on the front side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunneling oxide layer is 1.5 to 2.0 nm.
[0070] 42. According to the method described in item 39, the thickness of the polysilicon layer deposited on the front side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0071] 43. According to the method described in item 33, when the LPCVD method is used to form the back passivation layer and the front passivation layer, a tunneling oxide layer and a polysilicon layer are simultaneously deposited on the back and front sides of the silicon wafer to form the back passivation layer and the front passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0072] 44. According to the method described in item 43, the thickness of the tunneling oxide layer deposited on the back side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunneling oxide layer is 1.5 to 2.0 nm.
[0073] 45. According to the method described in item 43, the thickness of the polysilicon layer deposited on the back side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0074] 46. According to the method described in item 43, after a polysilicon layer is deposited on a silicon wafer, boron or phosphorus is doped into the polysilicon layer to form a doped polysilicon layer.
[0075] 47. According to the method described in item 43, after the back passivation layer is formed by LPCVD, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0076] 48. According to the method described in item 29, after the front side of the silicon wafer is cleaned, the silicon wafer is placed in a tubular diffusion furnace to perform annealing treatment on the silicon wafer.
[0077] 49. According to the method described in item 48, the temperature in the tubular diffusion furnace is 800-1200°C; preferably, the temperature in the tubular diffusion furnace is 900-1050°C.
[0078] 50. According to the method described in item 48, N2 is introduced into the tubular diffusion furnace; preferably, the flow rate of N2 is 5000-25000 sccm; further preferably, the flow rate of N2 is 10000-20000 sccm.
[0079] 51. According to the method described in item 48, H2 is introduced into the tubular diffusion furnace; preferably, the flow rate of H2 is 300-15000 sccm; further preferably, the flow rate of H2 is 500-10000 sccm.
[0080] 52. According to the method described in item 48, annealing is carried out in a tubular diffusion furnace for 30 to 240 minutes; preferably, annealing is carried out in a tubular diffusion furnace for 60 to 180 minutes.
[0081] 53. According to the method described in item 29, when depositing the anti-reflection layer, an aluminum oxide layer and a silicon nitride layer are deposited on the silicon wafer to form the anti-reflection layer; preferably, the aluminum oxide layer and the silicon nitride layer are deposited on the front and back sides of the silicon wafer at the same time; further preferably, the aluminum oxide layer is deposited on the silicon wafer first, and then the silicon nitride layer is deposited.
[0082] 54. According to the method described in item 53, when depositing the aluminum oxide layer, ALD equipment is used for deposition.
[0083] 55. According to the method described in item 53, the thickness of the deposited aluminum oxide layer is 1 to 15 nm; preferably, the thickness of the deposited aluminum oxide layer is 2 to 10 nm.
[0084] 56. According to the method described in item 53, when depositing the silicon nitride layer, a PECVD method is used for deposition.
[0085] 57. According to the method described in item 29, the thickness of the deposited silicon nitride layer is 40 to 120 nm; preferably, the thickness of the deposited silicon nitride layer is 60 to 100 nm.
[0086] 58. According to the method described in item 29, when making the metal grid line, the silver paste is printed on the front and back of the silicon wafer by screen printing.
[0087] Beneficial Effects
[0088] 1. The selective passivation contact structure in the present application forms a local passivation contact structure on the light-receiving surface only in the metallized contact area, which solves the problem of low conversion efficiency caused by parasitic absorption of the polysilicon film layer on the light-receiving surface;
[0089] 2. At the same time, limited by the increase in the number of gate lines, the excessive metallization area leads to excessive shading and low short-circuit current. This application can achieve passivation contact when there are more than 180 gate lines on a 182-size silicon wafer. Breaking the existing cell's dependence on selective emitter technology, that is, SE technology, compared to conventional laser SE technology, the selective passivation contact structure can be flexibly adjusted, and avoids the silicon-based loss caused by laser SE, has more matching structures, and has a large technical space. The realization of local selective passivation contact greatly increases the carrier absorption capacity of the non-metallic area on the cell.
[0090] 3. Local masking is achieved through laser technology, avoiding the problem of liquid contamination caused by existing acid / alkali resistant slurry. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] Figure 1 It is a schematic diagram of the solar cell structure of this application.
[0092] In the figure, 1. front gate line; 2. laminated anti-reflection film; 3. front aluminum oxide layer; 4. front polysilicon layer; 5. front tunneling layer; 6. substrate; 7. back tunneling layer; 8. back polysilicon layer; 9. back aluminum oxide layer; 10. silicon nitride anti-reflection film; 11. back gate line. DETAILED DESCRIPTION
[0093] The present application is described in detail below. Although specific embodiments of the present application are shown, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.
[0094] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the functional differences of components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" are open-ended terms and should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present application, but the description is based on the general principles of the specification and is not intended to limit the scope of the present application. The scope of protection of the present application shall be determined by the attached claims.
[0095] refer to Figure 1 , the present application provides a solar cell with a selective passivation contact structure, wherein the solar cell comprises a substrate, a second passivation layer is arranged on the substrate, and the second passivation layer is arranged on the front side of the substrate;
[0096] In the field of solar cells, the surface of a solar cell that is exposed to sunlight is called the front side; the side facing away from the front side is called the back side.
[0097] The substrate is a silicon-based substrate, and the substrate can be a P-type silicon wafer or an N-type silicon wafer.
[0098] In the present application, the substrate is a P-type silicon wafer.
[0099] In the present application, a second passivation layer is provided on the front side of the solar cell, and the second passivation layer can reduce the parasitic absorption of electrons, thereby solving the problem of low conversion rate caused by parasitic absorption; and increase the carrier absorption capacity of the solar cell in the non-metallic area, thereby improving the number of fill factors.
[0100] In the present application, the second passivation layer is disposed on the front side of the substrate, so that a small number of electrodes are disposed on the substrate to achieve the purpose of increasing the fill factor, reducing the impact of the sun's rays being blocked on the front side of the solar cell caused by the large number of electrodes, thereby achieving the goal of increasing the fill factor while ensuring the amount of light, and improving the conversion efficiency of solar energy.
[0101] The second passivation layer covers a local position of the substrate. Preferably, the second passivation layer covers a local position of the substrate where current or voltage exists. Further preferably, a front gate line is arranged on the substrate, and the second passivation layer is arranged between the front gate line and the substrate.
[0102] The second passivation layer is used to form a passivation contact structure between the substrate and the gate line, thereby reducing the parasitic absorption between the substrate and the gate line; thereby improving the carrier absorption capacity between the substrate and the gate line. Thus, the shading effect caused by increasing the fill factor by adding gate lines is solved. Therefore, the number of gate lines is controlled, thereby increasing the amount of sunlight on the substrate, and further improving the conversion efficiency of the solar cell.
[0103] Preferably, a first passivation layer is disposed on a side of the substrate facing away from the second passivation layer, that is, the first passivation layer is disposed on the back side of the substrate.
[0104] The first passivation layer has good corrosion resistance, so the first passivation layer has a protective effect on the substrate, which can reduce the possibility of corrosion and damage to the back of the substrate, thereby increasing the service life of the substrate and the solar cell.
[0105] The second passivation layer includes a tunneling layer; preferably, the second passivation layer also includes a doping layer; further preferably, the second passivation layer includes a tunneling layer and a doping layer stacked in sequence in a front direction.
[0106] The first passivation layer includes a tunneling layer. Preferably, the first passivation layer also includes a doping layer. Further preferably, the first passivation layer includes a tunneling layer and a doping layer stacked in sequence in a direction toward the back side.
[0107] The tunneling layer is a silicon oxide layer, and the doping layer is a polysilicon layer doped with phosphorus or boron.
[0108] The work function of the doping layer is different from that of the substrate, and an accumulation layer is generated at the interface between the doping layer and the substrate. The accumulation layer prevents holes from entering the tunneling layer and helps electrons enter the tunneling layer, thereby reducing the recombination loss of minority carriers, which is beneficial to improving the fill factor and obtaining a higher open circuit voltage.
[0109] The doping layers of the first passivation layer and the second passivation layer are doping layers with different doping; preferably, the doping layer of the first passivation layer is a boron-doped doping layer, and the doping layer of the second passivation layer is a phosphorus-doped doping layer, and further preferably, the doping layer of the first passivation layer is a boron-doped polysilicon layer, and the doping layer of the second passivation layer is a phosphorus-doped polysilicon layer.
[0110] Since the first passivation layer and the second passivation layer are respectively arranged on the two sides of the substrate. In the present application, the substrate is a P-type silicon wafer, which is formed by doping boron in silicon material. Therefore, a phosphorus-doped doping layer is used on the front side of the silicon wafer, so that a PN junction is formed between the doping layer on the front side and the substrate. The PN junction has a photovoltaic effect, which can excite electron-hole pairs with photons, thereby making the doped layer and the substrate conductive.
[0111] A first anti-reflection layer is arranged on the substrate, and the anti-reflection layer is used to improve the utilization of sunlight;
[0112] Preferably, a second anti-reflection layer is provided on the side of the substrate facing away from the first anti-reflection layer;
[0113] Further preferably, the first anti-reflection layer is arranged on a side of the first passivation layer away from the substrate; and the second anti-reflection layer is arranged on a side of the second passivation layer away from the substrate.
[0114] The first anti-reflection layer comprises an aluminum oxide layer, and the second anti-reflection layer comprises an aluminum oxide layer;
[0115] Preferably, the first anti-reflection layer comprises a silicon nitride anti-reflection film, and the second anti-reflection layer comprises a laminated anti-reflection film;
[0116] Further preferably, the first anti-reflection layer comprises a silicon nitride anti-reflection film and an aluminum oxide layer, and the second anti-reflection layer comprises a laminated anti-reflection film and an aluminum oxide layer;
[0117] Further preferably, the first anti-reflection layer is arranged on the back side of the substrate, and the second anti-reflection layer is arranged on the front side of the substrate.
[0118] The second anti-reflection layer is used to reduce the reflection of sunlight, thereby increasing the irradiation rate of sunlight on the solar cell, so the second anti-reflection layer is arranged on the front side of the substrate, so that sunlight can be more fully irradiated on the solar cell, thereby improving the conversion efficiency of the solar cell.
[0119] The first anti-reflection layer can not only reduce the reflection of sunlight, but also reflect the sunlight irradiated on the substrate back to the substrate, further improving the utilization rate of sunlight. The first anti-reflection layer located on the back of the substrate is located on the back of the substrate, so that the sunlight diffusely reflected by the environment can be more fully irradiated on the back of the substrate. At the same time, the first anti-reflection layer and the second anti-reflection layer will reflect the sunlight reflected and transmitted from the substrate back to the substrate, thereby improving the conversion rate of sunlight.
[0120] A back gate line is arranged on the substrate, and the back gate line and the first passivation layer are located on the same side. Preferably, the first passivation layer is located between the substrate and the back gate line.
[0121] The back grid line is arranged between the first passivation layer and the substrate, so that the first passivation layer can passivate between the back grid line and the substrate, thereby reducing the parasitic absorption of the doping layer, thereby improving the conversion efficiency of the solar cell to sunlight.
[0122] In summary, the present application provides a solar cell with selective passivation contact, wherein a second passivation layer is arranged on a substrate, and the second passivation layer is composed of a phosphorus-doped polysilicon layer and a silicon oxide layer. The selective passage of carriers can be achieved between the polysilicon layer and the silicon oxide layer, and between the silicon oxide layer and the polysilicon layer. The majority carriers can penetrate these two layers, while the minority carriers are blocked, thereby achieving passivation contact between the front side of the substrate and the gate line, thereby increasing the short-circuit voltage between the silicon wafer and the gate line, and improving the conversion efficiency of the battery. At the same time, the second passivation layer can also increase the number of fill factors to a limited extent, reduce the number of gate lines, and thereby reduce the amount of sunlight blocked by the gate lines, so as to achieve the purpose of improving the sunlight conversion efficiency.
[0123] The present application also provides a method for manufacturing a selective passivation contact structure, which includes:
[0124] Polish the silicon wafer on both sides.
[0125] Make the back passivation layer and the front passivation layer on the silicon wafer.
[0126] A mask layer is made locally on the front side of the silicon wafer.
[0127] Clean the mask layer on the front side of the silicon wafer and the passivation layer on the front side where the mask layer is not generated.
[0128] A selectively passivated contact structure is obtained;
[0129] When the mask layer is locally formed on the front side, the mask layer is formed at the position of the preset electrode.
[0130] In the present application, the substrate of the solar cell is a silicon wafer substrate.
[0131] Polishing both sides of the silicon wafer makes the surface easier to deposit.
[0132] The front passivation layer and the back passivation layer are deposited on the polished silicon wafer. The back passivation layer is used to protect the back of the silicon wafer and reduce the possibility of corrosion on the back of the silicon wafer. The front passivation layer is used to solve the parasitic absorption problem of the light-receiving surface, thereby improving the conversion efficiency.
[0133] The mask layer is a protective layer, which is arranged at a local position of the front side and is used to protect the front side passivation layer on the silicon wafer.
[0134] When the front side of the silicon wafer is cleaned, the passivation layer on the front side will be cleaned off. At the same time, since the mask layer arranged at a part of the silicon wafer and the front passivation layer can protect the passivation layer, after cleaning the front side of the silicon wafer, a silicon wafer having a passivation contact structure partially covered on the front side is obtained.
[0135] The passivation contact structure on the front side of the silicon wafer is set at the position of the preset electrode. The passivation structure can realize the selective passage of carriers. The majority carriers can penetrate these two layers, while the minority carriers are blocked. This can realize the passivation contact between the front side of the silicon wafer and the electrode, thereby improving the conversion efficiency of the battery.
[0136] The mask layer is a silicon oxide mask layer.
[0137] The silicon oxide mask layer has high selectivity, does not react with chemicals and gases, and can prevent the diffusion of doping substances such as boron and phosphorus, so that a precisely controlled edge area can be obtained.
[0138] When the mask layer is formed, a laser method is used to form the mask layer.
[0139] Laser is used to irradiate the silicon wafer, causing the surface of the silicon wafer to react with air or oxygen to form silicon oxide, thereby forming a silicon oxide mask layer on the surface of the silicon wafer.
[0140] When manufacturing the back passivation layer and the front passivation layer, the LPCVD method and / or the PECVD method are used.
[0141] When manufacturing the back passivation layer and the front passivation layer, the back passivation layer is manufactured first and then the front passivation layer is manufactured.
[0142] In a specific embodiment, when the back passivation layer is made by PECVD, a tunnel oxide layer and a polysilicon layer are deposited on the back of the silicon wafer to form the back passivation layer. Preferably, the tunnel oxide layer is deposited first and then the polysilicon layer is deposited.
[0143] The work function of polysilicon layers is different from that of silicon wafers. An accumulation layer is generated at the interface between the polysilicon layer and the silicon wafer. The accumulation layer prevents holes from entering the tunneling oxide layer and helps electrons enter the tunneling oxide layer. The tunneling silicon oxide layer has good compactness and good surface passivation. This reduces the recombination loss of minority carriers, helps to improve the fill factor, and obtain a higher open circuit voltage, further improving the conversion efficiency of solar cells.
[0144] The polysilicon layer deposited on the back of the silicon wafer is a boron-doped polysilicon layer.
[0145] In this application, a P-type silicon wafer is selected as the silicon wafer. Therefore, in order to reduce the resistance between the back polysilicon layer and the silicon wafer and also prevent the possibility of a PN junction between the polysilicon layer and the silicon wafer, a boron-doped polysilicon layer is prepared on the back of the silicon wafer.
[0146] On the front side of the silicon wafer, a passivation layer is set to solve the problem of low conversion efficiency caused by parasitic absorption on the light-receiving surface. Therefore, a phosphorus-doped polysilicon layer is deposited on the silicon wafer to increase the resistance between the polysilicon layer and the silicon wafer, which can effectively increase the fill factor and increase the short-circuit current, thereby improving the conversion efficiency.
[0147] The thickness of the tunnel oxide layer deposited on the back of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunnel oxide layer is 1.5 to 2.0 nm.
[0148] The deposition thickness of the back tunneling oxide layer is: 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, and 3nm.
[0149] The thickness of the polysilicon layer deposited on the back of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0150] The thickness of the back polysilicon layer is: 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, and 300nm.
[0151] After the back passivation layer is formed by the PECVD method, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0152] The polysilicon layer of the front passivation layer and the polysilicon layer of the back passivation layer are phosphorus-doped polysilicon layers and boron-doped polysilicon layers, respectively. Since the polysilicon layers of the front passivation layer and the back passivation layer are layers of different materials, the passivation layer on the front side of the back passivation layer is cleaned to be removed, and then the front passivation layer is deposited on the front side of the silicon wafer.
[0153] When the front passivation layer is manufactured by the PECVD method, a tunneling layer and a polysilicon layer are deposited on the front side of the silicon wafer to form the front passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0154] The use of tunneling oxide layer and polysilicon layer can achieve selective passage of carriers. Majority carriers can penetrate these two layers, while minority carriers are blocked. This can achieve passivation contact between the front side of the silicon wafer and the gate line, thereby improving the conversion efficiency of the battery.
[0155] The thickness of the tunnel oxide layer deposited on the front side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunnel oxide layer is 1.5 to 2.0 nm.
[0156] The deposition thickness of the front tunneling oxide layer is: 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, and 3nm.
[0157] The thickness of the polysilicon layer deposited on the front side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0158] The thickness of the front polysilicon layer deposited is: 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, and 300nm.
[0159] In another specific embodiment, the passivation layer is prepared using a LPCVD method.
[0160] When the back passivation layer and the front passivation layer are made by the LPCVD method, a tunneling oxide layer and a polysilicon layer are deposited on the back and front of the silicon wafer to form the back passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0161] After polysilicon is deposited on a silicon wafer, boron or phosphorus is then doped onto the polysilicon layer to dope the polysilicon layer.
[0162] When the passivation layer is prepared using the LPCVD method, a tunneling oxide layer and a polysilicon layer are directly formed on the upper and lower sides of the silicon wafer, and then the polysilicon layer on the front and back sides of the silicon wafer is doped respectively to form doped polysilicon layers.
[0163] The doped polysilicon layer and the tunnel oxide layer work together to form a passivation layer of the passivation structure.
[0164] The use of LPCVD to prepare the passivation layer can simultaneously form the passivation layer on the front and back sides of the silicon wafer, simplifying the manufacturing process of the passivation structure on the silicon wafer and making the preparation of the front and back passivation layers on the silicon wafer more convenient.
[0165] After the back passivation layer is formed by the LPCVD method, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0166] The silicon wafer with the tunnel oxide layer and the polysilicon layer formed thereon is placed in a high temperature furnace for boron diffusion, so that a boron-doped polysilicon layer is formed on the back side of the silicon wafer.
[0167] Since part of the boron will diffuse to the front side of the silicon wafer when the high temperature furnace is used for diffusion, a chain cleaning machine is used to clean the polysilicon layer that diffuses to the front side of the silicon wafer and forms a boron-doped layer.
[0168] After the back passivation layer is made using the LPCVD method, phosphorus is diffused on the front side of the silicon wafer to form a front passivation layer.
[0169] The polysilicon layer on the front side of the silicon wafer is doped with phosphorus, thereby forming a phosphorus-doped polysilicon layer on the front side of the silicon wafer.
[0170] The doped polysilicon layer on the front of the silicon wafer will form a PN junction with the silicon wafer, further increasing the resistance between the silicon wafer and the passivation layer, thereby increasing the short-circuit voltage on the silicon wafer and achieving the purpose of improving conversion efficiency.
[0171] The thickness of the tunnel oxide layer deposited on the back of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunnel oxide layer is 1.5 to 2.0 nm.
[0172] The deposition thickness of the back tunneling oxide layer is: 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, and 3nm.
[0173] The thickness of the polysilicon layer deposited on the back of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0174] The thickness of the back polysilicon layer deposited is: 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, and 300nm.
[0175] In summary, the present application provides a method for manufacturing a selective passivation contact structure, in which a front passivation layer is prepared on the front side of a silicon wafer, and the front passivation layer is composed of a tunneling oxide layer and a polysilicon layer. The tunneling oxide layer and the polysilicon layer can realize the selective passage of carriers, and majority carriers can penetrate these two layers, while minority carriers are blocked, thereby realizing the passivation contact between the front side of the silicon wafer and the electrode, thereby increasing the short-circuit voltage between the silicon wafer and the electrode, and improving the conversion efficiency of the battery. In the preparation process, a front passivation layer is first deposited on the front side of the silicon wafer, and then a mask layer is deposited on the upper surface of the front passivation layer that needs to be retained, and then the mask layer and the front passivation layer without the mask layer deposited are cleaned, and the front passivation layer with the deposited mask layer is retained. The front passivation layer prepared by this method has a clear boundary. The transition between the silicon wafer and the front side can be clearer.
[0176] The present application also provides a method for preparing a solar cell with a selectively passivated contact structure, wherein:
[0177] Polish the silicon wafer on both sides.
[0178] Make the back passivation layer and the front passivation layer on the silicon wafer.
[0179] A mask layer is made locally on the front side of the silicon wafer.
[0180] Silicon wafer front cleaning,
[0181] Depositing an anti-reflection layer on the silicon wafer,
[0182] Making gate lines on silicon wafers,
[0183] Inject light into silicon wafers and / or sinter them to obtain solar cells;
[0184] When the mask layer is locally formed on the front surface, the mask layer is formed at the position of the preset gate line.
[0185] The mask layer is a silicon oxide mask layer and is manufactured by a laser method.
[0186] When manufacturing the back passivation layer and the front passivation layer, the back passivation layer is manufactured first and then the front passivation layer is manufactured.
[0187] In the present application, the substrate of the solar cell is a silicon wafer substrate.
[0188] Polishing both sides of the silicon wafer makes the surface easier to deposit.
[0189] The front passivation layer and the back passivation layer are deposited on the polished silicon wafer. The back passivation layer is used to protect the back of the silicon wafer and reduce the possibility of corrosion on the back of the silicon wafer. The front passivation layer is used to solve the parasitic absorption problem of the light-receiving surface, thereby improving the conversion efficiency.
[0190] The mask layer is a protective layer, which is arranged at a local position of the front side and is used to protect the front side passivation layer on the silicon wafer.
[0191] When the front side of the silicon wafer is cleaned, the passivation layer on the front side will be cleaned off. At the same time, since the mask layer arranged at a part of the silicon wafer and the front passivation layer can protect the passivation layer, after cleaning the front side of the silicon wafer, a silicon wafer having a passivation contact structure partially covered on the front side is obtained.
[0192] The passivation contact structure on the front side of the silicon wafer is set at the position of the preset electrode. The passivation structure can realize the selective passage of carriers. The majority carriers can penetrate these two layers, while the minority carriers are blocked. This can realize the passivation contact between the front side of the silicon wafer and the electrode, thereby improving the conversion efficiency of the battery.
[0193] The mask layer is a silicon oxide mask layer.
[0194] The silicon oxide mask layer has high selectivity, does not react with chemicals and gases, and can prevent the diffusion of doping substances such as boron and phosphorus, so that a precisely controlled edge area can be obtained.
[0195] When the mask layer is formed, a laser method is used to form the mask layer.
[0196] Laser is used to irradiate the silicon wafer, causing the surface of the silicon wafer to react with air or oxygen to form silicon oxide, thereby forming a silicon oxide mask layer on the surface of the silicon wafer.
[0197] When manufacturing the back passivation layer and the front passivation layer, the LPCVD method and / or the PECVD method are used.
[0198] When manufacturing the back passivation layer and the front passivation layer, the back passivation layer is manufactured first and then the front passivation layer is manufactured.
[0199] In a specific embodiment, when the back passivation layer is made by PECVD, a tunnel oxide layer and a polysilicon layer are deposited on the back of the silicon wafer to form the back passivation layer. Preferably, the tunnel oxide layer is deposited first and then the polysilicon layer is deposited.
[0200] The work function of polysilicon layers is different from that of silicon wafers. An accumulation layer is generated at the interface between the polysilicon layer and the silicon wafer. The accumulation layer prevents holes from entering the tunneling oxide layer and helps electrons enter the tunneling oxide layer. The tunneling silicon oxide layer has good compactness and good surface passivation. This reduces the recombination loss of minority carriers, helps to improve the fill factor, and obtain a higher open circuit voltage, further improving the conversion efficiency of solar cells.
[0201] The polysilicon layer deposited on the back of the silicon wafer is a boron-doped polysilicon layer.
[0202] In this application, a P-type silicon wafer is selected as the silicon wafer. Therefore, in order to reduce the resistance between the back polysilicon layer and the silicon wafer and also prevent the possibility of a PN junction between the polysilicon layer and the silicon wafer, a boron-doped polysilicon layer is prepared on the back of the silicon wafer.
[0203] On the front side of the silicon wafer, a passivation layer is set to solve the problem of low conversion efficiency caused by parasitic absorption on the light-receiving surface. Therefore, a phosphorus-doped polysilicon layer is deposited on the silicon wafer to increase the resistance between the polysilicon layer and the silicon wafer, which can effectively increase the fill factor and increase the short-circuit current, thereby improving the conversion efficiency.
[0204] The thickness of the tunnel oxide layer deposited on the back of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunnel oxide layer is 1.5 to 2.0 nm.
[0205] The deposition thickness of the back tunneling oxide layer is: 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, and 3nm.
[0206] The thickness of the polysilicon layer deposited on the back of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0207] The thickness of the back polysilicon layer is: 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, and 300nm.
[0208] After the back passivation layer is formed by the PECVD method, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0209] The polysilicon layer of the front passivation layer and the polysilicon layer of the back passivation layer are phosphorus-doped polysilicon layers and boron-doped polysilicon layers, respectively. Since the polysilicon layers of the front passivation layer and the back passivation layer are layers of different materials, the passivation layer on the front side of the back passivation layer is cleaned to be removed, and then the front passivation layer is deposited on the front side of the silicon wafer.
[0210] When the front passivation layer is manufactured by the PECVD method, a tunneling layer and a polysilicon layer are deposited on the front side of the silicon wafer to form the front passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0211] The use of tunneling oxide layer and polysilicon layer can achieve selective passage of carriers. Majority carriers can penetrate these two layers, while minority carriers are blocked. This can achieve passivation contact between the front side of the silicon wafer and the gate line, thereby improving the conversion efficiency of the battery.
[0212] The thickness of the tunnel oxide layer deposited on the front side of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunnel oxide layer is 1.5 to 2.0 nm.
[0213] The deposition thickness of the front tunneling oxide layer is: 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, and 3nm.
[0214] The thickness of the polysilicon layer deposited on the front side of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0215] The thickness of the front polysilicon layer deposited is: 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, and 300nm.
[0216] In another specific embodiment, the passivation layer is prepared using a LPCVD method.
[0217] When the back passivation layer and the front passivation layer are made by the LPCVD method, a tunneling oxide layer and a polysilicon layer are deposited on the back and front of the silicon wafer to form the back passivation layer. Preferably, the tunneling oxide layer is deposited first and then the polysilicon layer is deposited.
[0218] After polysilicon is deposited on a silicon wafer, boron or phosphorus is then doped onto the polysilicon layer to dope the polysilicon layer.
[0219] When the passivation layer is prepared using the LPCVD method, a tunneling oxide layer and a polysilicon layer are directly formed on the upper and lower sides of the silicon wafer, and then the polysilicon layer on the front and back sides of the silicon wafer is doped respectively to form doped polysilicon layers.
[0220] The doped polysilicon layer and the tunnel oxide layer work together to form a passivation layer of the passivation structure.
[0221] The use of LPCVD to prepare the passivation layer can simultaneously form the passivation layer on the front and back sides of the silicon wafer, simplifying the manufacturing process of the passivation structure on the silicon wafer and making the preparation of the front and back passivation layers on the silicon wafer more convenient.
[0222] After the back passivation layer is formed by the LPCVD method, the front side of the silicon wafer is cleaned; preferably, a chain cleaning machine is used to clean the front side of the silicon wafer.
[0223] The silicon wafer with the tunnel oxide layer and the polysilicon layer formed thereon is placed in a high temperature furnace for boron diffusion, so that a boron-doped polysilicon layer is formed on the back side of the silicon wafer.
[0224] Since part of the boron will diffuse to the front side of the silicon wafer when the high temperature furnace is used for diffusion, a chain cleaning machine is used to clean the polysilicon layer that diffuses to the front side of the silicon wafer and forms a boron-doped layer.
[0225] After the back passivation layer is made using the LPCVD method, phosphorus is diffused on the front side of the silicon wafer to form a front passivation layer.
[0226] The polysilicon layer on the front side of the silicon wafer is doped with phosphorus, thereby forming a phosphorus-doped polysilicon layer on the front side of the silicon wafer.
[0227] The doped polysilicon layer on the front of the silicon wafer will form a PN junction with the silicon wafer, further increasing the resistance between the silicon wafer and the passivation layer, thereby increasing the short-circuit voltage on the silicon wafer and achieving the purpose of improving conversion efficiency.
[0228] The thickness of the tunnel oxide layer deposited on the back of the silicon wafer is 1 to 3 nm; preferably, the thickness of the tunnel oxide layer is 1.5 to 2.0 nm.
[0229] The deposition thickness of the back tunneling oxide layer is: 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, and 3nm.
[0230] The thickness of the polysilicon layer deposited on the back of the silicon wafer is 20 to 300 nm; preferably, the thickness of the polysilicon layer is 50 to 200 nm.
[0231] The thickness of the back polysilicon layer deposited is: 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, and 300nm.
[0232] After the front side of the silicon wafer is cleaned, the silicon wafer is placed in a tubular diffusion furnace for annealing.
[0233] The temperature in the tubular diffusion furnace is 800-1200°C; preferably, the temperature in the tubular diffusion furnace is 900-1050°C.
[0234] Specifically, the temperatures in the tubular diffusion furnace are: 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, and 1200°C.
[0235] N2 is introduced into the tubular diffusion furnace; preferably, the flow rate of N2 is 5000-25000 sccm; further preferably, the flow rate of N2 is 10000-20000 sccm.
[0236] When annealing is performed in a tubular diffusion furnace, nitrogen is introduced into the tubular diffusion furnace so that the silicon wafer is annealed in nitrogen.
[0237] Specifically, the flow rate of N2 is: 5000sccm, 6000sccm, 7000sccm, 8000sccm, 9000sccm, 10000sccm, 11000sccm, 12000sccm, 13000sccm, 14000sccm, 15000sccm, 16000sccm, 17000sccm, 18000sccm, 19000sccm, 20000sccm, 21000sccm, 22000sccm, 23000sccm, 24000sccm, and 25000sccm.
[0238] H2 is introduced into the tubular diffusion furnace; preferably, the flow rate of H2 is 300-15000 sccm; further preferably, the flow rate of H2 is 500-10000 sccm.
[0239] When annealing in a tubular diffusion furnace, hydrogen is introduced at the same time as nitrogen, that is, hydrogen and nitrogen are introduced into the tubular annealing furnace at the same time to anneal the silicon wafer.
[0240] Specifically, the flow rate of H2 is: 300sccm, 400sccm, 500sccm, 600sccm, 700sccm, 800sccm, 900sccm, 1000sccm, 1100sccm, 1200sccm, 1300sccm, 1400sccm, 1500sccm, 1600sccm, 1700sccm, 1800sccm, 1900sccm, 2000sccm, 2500sccm, 3000sccm ccm, 3500sccm, 4000sccm, 4500sccm, 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm, 8000s ccm, 8500sccm, 9000sccm, 9500sccm, 10000sccm, 11000sccm, 12000sccm, 13000sccm, 14000sccm, 15000sccm.
[0241] The annealing is performed in a tubular diffusion furnace for 30 to 240 minutes; preferably, the annealing is performed in a tubular diffusion furnace for 60 to 180 minutes.
[0242] Specifically, the annealing time in the tubular diffusion furnace is: 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min, 130min, 140min, 150min, 160min, 170min, 180min, 190min, 200min, 210min, 220min, 230min, and 240min.
[0243] When depositing the anti-reflection layer, an aluminum oxide layer and a silicon nitride layer are deposited on the silicon wafer to form the anti-reflection layer; preferably, the aluminum oxide layer and the silicon nitride layer are deposited on the front and back sides of the silicon wafer at the same time; further preferably, the aluminum oxide layer is first deposited on the silicon wafer, and then the silicon nitride layer is deposited.
[0244] In a specific embodiment, when depositing the aluminum oxide layer, an ALD device is used for deposition.
[0245] The thickness of the deposited aluminum oxide layer is 1 to 15 nm; preferably, the thickness of the deposited aluminum oxide layer is 2 to 10 nm.
[0246] Specifically, the thickness of the deposited aluminum oxide layer is: 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, and 15 nm.
[0247] In a specific embodiment, when depositing the silicon nitride layer, a PECVD method is used for deposition.
[0248] The thickness of the deposited silicon nitride layer is 40-120 nm; preferably, the thickness of the deposited silicon nitride layer is 60-100 nm.
[0249] The thickness of the deposited silicon nitride layer is: 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, and 120nm.
[0250] When making metal grid lines, screen printing is used to print silver paste on the front and back of the silicon wafer.
[0251] In summary, the present application provides a method for preparing a solar cell with a selective passivation contact structure, wherein a front passivation layer is prepared on the front of a silicon wafer, and the front passivation layer is composed of a tunneling oxide layer and a polysilicon layer, and the selective passage of carriers can be realized between the tunneling oxide layer and the polysilicon layer, and the majority carriers can penetrate these two layers, while the minority carriers are blocked, thereby realizing the passivation contact between the front of the silicon wafer and the electrode, thereby increasing the short-circuit voltage between the silicon wafer and the electrode, and improving the conversion efficiency of the battery. In the preparation process, a front passivation layer is first deposited on the front of the silicon wafer, and then a mask layer is deposited on the upper surface of the front passivation layer to be retained, and then the mask layer and the front passivation layer without the mask layer deposited are cleaned, and the front passivation layer with the mask layer deposited is retained. The front passivation layer prepared by this method has a clear boundary. The transition between the silicon wafer and the front is clearer. Anti-reflection layers are deposited on the front and back of the silicon wafer to reduce the reflection and refraction of sunlight, further reduce the waste of sunlight, and improve the conversion efficiency of sunlight.
[0252] Example 1
[0253] 1) Select the original P-type silicon wafer as the silicon wafer substrate (hereinafter referred to as the silicon wafer), the silicon wafer is a 182-inch silicon wafer. After the texturing process, the silicon wafer is textured on both sides to form a pyramid-shaped texture surface on the surface of the silicon wafer;
[0254] 2) The silicon wafer after texturing is subjected to an alkali polishing process to polish both sides of the silicon wafer to form a tower base-shaped polished surface;
[0255] 3) The polished silicon wafer is subjected to a PECVD process to deposit a 1.5-2.0 nm silicon oxide tunneling layer and a 50-200 nm boron-doped polysilicon layer on the back of the silicon wafer;
[0256] 4) Use a chain cleaning machine to clean the polysilicon layer wrapped around the front of the silicon wafer, and at the same time, perform texturing on the front of the silicon wafer to form a pyramid morphology on the surface of the silicon wafer;
[0257] 5) The front side of the silicon wafer is subjected to a PECVD process to deposit a 1.5-2.0 nm silicon oxide tunneling layer and a 50-200 nm phosphorus-doped polysilicon layer on the front side of the silicon wafer.
[0258] 6) Using laser to make a local gate finger-shaped silicon oxide mask layer at the position of the preset electrode on the front side of the silicon wafer;
[0259] 7) The polysilicon layer and the protective mask layer are removed through a tank cleaning machine.
[0260] 8) Place the silicon wafer in a high temperature tubular diffusion furnace and anneal for 60-180 min at a high temperature of 900-1050°C, a N2 flow rate of 10000-20000sccm, and a H2 flow rate of 500-10000sccm.
[0261] 9) Place the silicon wafer in the ALD equipment and deposit a 2-10 nm aluminum oxide layer on both sides of the silicon wafer.
[0262] 10) Depositing silicon nitride layers on the front and back sides of the silicon wafer by PECVD, wherein the thickness of the silicon nitride layer is 60-100 nm.
[0263] 11) Use screen printing to apply silver paste on the front and back sides of the silicon wafer to form front and back metal grid lines. There are 180 grid lines on the front side and 190 grid lines on the back side. The grid lines are used to transmit current.
[0264] 12) Finally, through light injection equipment and laser sintering technology, the silicon wafer and the gate line form ohmic contact.
[0265] 13) Make solar cells and test their efficiency.
[0266] Example 2
[0267] 1) Select the original P-type silicon wafer as the silicon wafer substrate (hereinafter referred to as the silicon wafer), the silicon wafer is a 182-inch silicon wafer. After the texturing process, the silicon wafer is textured on both sides to form a pyramid-shaped texture surface on the surface of the silicon wafer;
[0268] 2) The silicon wafer after texturing is subjected to an alkali polishing process to polish both sides of the silicon wafer to form a tower base-shaped polished surface;
[0269] 3) The polished silicon wafer is subjected to the LPCVD process to deposit a 1.5-2.0nm silicon oxide tunneling layer and a 50-200nm polysilicon layer on the back and front of the silicon wafer respectively.
[0270] 4) Placing the silicon wafer in a high-temperature diffusion furnace for boron diffusion to form a boron-doped polysilicon layer on the back of the silicon wafer;
[0271] 5) The chain cleaning machine cleans the boron-doped polysilicon layer formed by plating on the front side of the silicon wafer, and at the same time, texturing the front side of the silicon wafer to form a pyramid morphology on the front side of the silicon wafer;
[0272] 6) Placing the silicon wafer in a high-temperature diffusion furnace for phosphorus diffusion, so that a phosphorus-doped polysilicon layer is formed on the front side of the silicon wafer, a PN junction is formed on the front side of the silicon wafer, and an N-type semiconductor is formed on the front side of the silicon wafer.
[0273] 7) Using laser to make a local gate finger-shaped silicon oxide mask layer at the position of the preset electrode on the front side of the silicon wafer;
[0274] 8) The polysilicon layer and the protective mask layer are removed through a tank cleaning machine.
[0275] 9) Place the silicon wafer in a high temperature tubular diffusion furnace and anneal for 60-180 min at a high temperature of 900-1050°C, a N2 flow rate of 10000-20000sccm, and a H2 flow rate of 500-10000sccm.
[0276] 10) Place the silicon wafer in an ALD device and deposit a 2-10 nm aluminum oxide layer on both sides of the silicon wafer.
[0277] 11) A silicon nitride layer is deposited on the front and back sides of the silicon wafer by PECVD method, wherein the thickness of the silicon nitride layer is 60-100 nm.
[0278] 12) Use screen printing to apply silver paste on the front and back sides of the silicon wafer to form front and back metal grid lines. There are 180 grid lines on the front side and 190 grid lines on the back side. The grid lines are used to transmit current.
[0279] 13) Finally, through light injection equipment and laser sintering technology, the silicon wafer and the gate line form ohmic contact.
[0280] 14) Make solar cells and test their efficiency.
[0281] Comparative Example 1
[0282] 1) Select the original P-type silicon wafer as the silicon wafer substrate (hereinafter referred to as the silicon wafer), the silicon wafer is a 182-inch silicon wafer. After the texturing process, the silicon wafer is textured on both sides to form a pyramid-shaped texture surface on the surface of the silicon wafer;
[0283] 2) The silicon wafer after texturing is subjected to an alkali polishing process to polish both sides of the silicon wafer to form a tower base-shaped polished surface;
[0284] 3) The polished silicon wafer is subjected to a PECVD process to deposit a 1.5-2.0 nm silicon oxide tunneling layer and a 50-200 nm boron-doped polysilicon layer on the back of the silicon wafer;
[0285] 4) Use a chain cleaning machine to clean the polysilicon layer wrapped around the front of the silicon wafer, and at the same time, perform texturing on the front of the silicon wafer to form a pyramid morphology on the surface of the silicon wafer;
[0286] 5) Use SE technology to passivate the front side of the silicon wafer;
[0287] 6) Place the silicon wafer in a high temperature tubular diffusion furnace and anneal for 60-180 min at a high temperature of 900-1050°C, a N2 flow rate of 10000-20000sccm, and a H2 flow rate of 500-10000sccm.
[0288] 7) Place the silicon wafer in the ALD equipment and deposit a 2-10 nm aluminum oxide layer on both sides of the silicon wafer.
[0289] 8) Depositing silicon nitride layers on the front and back sides of the silicon wafer by PECVD, wherein the thickness of the silicon nitride layer is 60-100 nm.
[0290] 9) Use screen printing to apply silver paste on the front and back sides of the silicon wafer to form front and back metal grid lines. There are 180 grid lines on the front side and 190 grid lines on the back side. The grid lines are used to transmit current.
[0291] 10) Finally, through light injection equipment and laser sintering technology, the silicon wafer and the gate line form ohmic contact.
[0292] 11) Make solar cells and test their efficiency.
[0293] Table 1
[0294] Example 1 Example 2 Comparative Example 1 Improved efficiency 0.04% 0.03% 0% The photoelectric conversion efficiency of the battery 26.64% 26.63% 26.60%
[0295] Comparative Example 2
[0296] 1) Select an original P-type silicon wafer as a silicon wafer substrate (hereinafter referred to as a silicon wafer), and the silicon wafer is a 182-inch silicon wafer. After a texturing process, the silicon wafer is textured on both sides to form a pyramid-shaped texture surface on the surface of the silicon wafer;
[0297] 2) The silicon wafer after texturing is subjected to an alkali polishing process to polish both sides of the silicon wafer to form a tower base-shaped polished surface;
[0298] 3) The polished silicon wafer is subjected to a PECVD process to deposit a 1.5-2.0 nm silicon oxide tunneling layer and a 50-200 nm boron-doped polysilicon layer on the back of the silicon wafer;
[0299] 4) Use a chain cleaning machine to clean the polysilicon layer wrapped around the front of the silicon wafer, and at the same time, perform texturing on the front of the silicon wafer to form a pyramid morphology on the surface of the silicon wafer;
[0300] 5) Use SE technology to passivate the front side of the silicon wafer;
[0301] 6) Place the silicon wafer in a high temperature tubular diffusion furnace and anneal for 60-180 min at a high temperature of 900-1050°C, a N2 flow rate of 10000-20000sccm, and a H2 flow rate of 500-10000sccm.
[0302] 7) Place the silicon wafer in the ALD equipment and deposit a 2-10 nm aluminum oxide layer on both sides of the silicon wafer.
[0303] 8) Depositing silicon nitride layers on the front and back sides of the silicon wafer by PECVD, wherein the thickness of the silicon nitride layer is 60-100 nm.
[0304] 9) Use screen printing to apply silver paste on the front and back sides of the silicon wafer to form front and back metal grid lines. There are 190 grid lines on the front side and 200 grid lines on the back side. The grid lines are used to transmit current.
[0305] 10) Finally, through light injection equipment and laser sintering technology, the silicon wafer and the gate line form ohmic contact.
[0306] 11) Make solar cells and test their efficiency.
[0307] Example 1 Example 2 Comparative Example 2 Improved efficiency 0.03% 0.02% 0% The photoelectric conversion efficiency of the battery 26.64% 26.63% 26.61%
[0308] The present application provides a solar cell with a selective passivation contact structure. By forming a local passivation contact structure in the metallized contact area on the light-receiving surface of the silicon wafer, the parasitic absorption problem of the polysilicon film layer is solved, thereby increasing the absorption capacity of carriers on the cell, solving the shading problem caused by too many gate lines, and achieving the purpose of improving the light conversion efficiency of the cell. Compared with conventional laser SE technology, the selective passivation contact structure can be flexibly adjusted, and avoids the silicon-based loss caused by laser SE, has more matching structures, and has a large technical space. In this application, local passivation technology is used on the light-receiving surface, and the conversion efficiency reaches 26.63% to 26.64%. The cell prepared in Example 1 increases by 0.04% compared with the existing cell. As the conversion efficiency of existing solar cells is close to the theoretical limit, this 0.04% increase is also very important for improving the light conversion efficiency of solar cells.
[0309] Referring to Comparative Examples 1 and 2, it can be seen that when the number of grid lines of existing conventional cells increases, the light conversion efficiency will also increase accordingly, but it also increases the blocking of sunlight, so the number of grid lines cannot be increased endlessly. Therefore, the present application sets a passivation layer at a local position so that the light conversion efficiency is improved while the number of grid lines does not increase. More importantly, the conversion efficiency of the cell using the passivation layer structure of the present application is also higher than the efficiency of the conventional cell after adding grid lines.
[0310] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A solar cell with a selectively passivated contact structure, wherein: The solar cell comprises a substrate, a second passivation layer is arranged on the substrate, and the second passivation layer is arranged on the front side of the substrate; Preferably, a first passivation layer is arranged on a side of the substrate facing away from the second passivation layer.
2. According to the solar cell according to claim 1, the second passivation layer covers a local position of the substrate. Preferably, the second passivation layer covers a local position of the substrate where current or voltage exists. Further preferably, a front grid line is arranged on the substrate, and the second passivation layer is arranged between the front grid line and the substrate.
3. According to the solar cell of claim 1 or 2, the second passivation layer comprises a tunneling layer; preferably, the second passivation layer further comprises a doping layer; further preferably, the second passivation layer comprises a tunneling layer and a doping layer stacked sequentially in a front direction.
4. According to the solar cell according to any one of claims 1 to 3, the first passivation layer includes a tunneling layer, preferably, the first passivation layer also includes a doping layer; further preferably, the first passivation layer includes a tunneling layer and a doping layer stacked in sequence in a direction toward the back side.
5. According to the solar cell according to any one of claims 1 to 4, the doping layers of the first passivation layer and the second passivation layer are doping layers with different doping; preferably, the doping layer of the first passivation layer is a boron-doped doping layer, and the doping layer of the second passivation layer is a phosphorus-doped doping layer, and further preferably, the doping layer of the first passivation layer is a boron-doped polycrystalline silicon layer, and the doping layer of the second passivation layer is a phosphorus-doped polycrystalline silicon layer.
6. The solar cell according to any one of claims 1 to 5, wherein a first anti-reflection layer is disposed on the substrate, and the anti-reflection layer is used to improve the utilization of sunlight; Preferably, a second anti-reflection layer is provided on the side of the substrate facing away from the first anti-reflection layer; Further preferably, the first anti-reflection layer is arranged on a side of the first passivation layer away from the substrate; and the second anti-reflection layer is arranged on a side of the second passivation layer away from the substrate.
7. The solar cell according to claim 6, wherein the first anti-reflection layer comprises an aluminum oxide layer, and the second anti-reflection layer comprises an aluminum oxide layer; Preferably, the first anti-reflection layer comprises a silicon nitride anti-reflection film, and the second anti-reflection layer comprises a laminated anti-reflection film; Further preferably, the first anti-reflection layer comprises a silicon nitride anti-reflection film and an aluminum oxide layer, and the second anti-reflection layer comprises a laminated anti-reflection film and an aluminum oxide layer; Further preferably, the first anti-reflection layer is arranged on the back side of the substrate, and the second anti-reflection layer is arranged on the front side of the substrate.
8. The solar cell according to any one of claims 1 to 7, wherein a back grid line is arranged on the substrate, the back grid line and the first passivation layer are located on the same side, and preferably, the first passivation layer is located between the substrate and the back grid line.
9. A method for manufacturing a selectively passivated contact structure, wherein: Polish the silicon wafer on both sides. Make the back passivation layer and the front passivation layer on the silicon wafer. A mask layer is locally made on the front side of the silicon wafer. Clean the mask layer on the front side of the silicon wafer and the passivation layer on the front side where the mask layer is not generated. A selectively passivated contact structure is obtained; When the mask layer is locally formed on the front side, the mask layer is formed at the position of the preset electrode.
10. A method for selectively passivating a contact structure of a solar cell, wherein: Polish the silicon wafer on both sides. Make the back passivation layer and the front passivation layer on the silicon wafer. A mask layer is locally made on the front side of the silicon wafer. Clean the mask layer on the front side of the silicon wafer and the passivation layer on the front side where the mask layer is not generated. Depositing an anti-reflection layer on the silicon wafer, Make gate lines on silicon wafers. Inject light into silicon wafers and / or sinter them to obtain solar cells; When the mask layer is locally formed on the front surface, the mask layer is formed at the position of the preset gate line.
Citation Information
Cited By
Back contact solar cell and short-process preparation method thereof
CN119342931A
A back contact solar cell and a short process preparation method thereof
CN119342931B