Positive plate, preparation method thereof and mixed ion battery
By adding lithium-containing active material layer and polymer to the potassium-containing active material layer of the positive electrode sheet of the potassium-ion battery, the challenges of potassium-ion battery in terms of energy density and cycle life are solved, and high energy density and good cycle performance are achieved. .
Patent Information
- Application Number
- CN202411429169.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-14
AI Technical Summary
Potassium ion batteries have challenges in energy density and cycle life, including narrow voltage windows, electrode dissolution, corrosion and by-products, resulting in poor cycle stability and short circuits, limiting the effective storage of K+.
A positive electrode sheet is designed, including a lithium-containing active material layer and a polymer on the surface of the potassium-containing active material layer, avoiding air corrosion through the polymer, and improving circulation performance and energy density through the lithium-potassium ion synergistic effect.
It effectively avoids material corrosion and side reactions, improves circulation performance and energy density, simplifies the preparation process, and improves the manufacturability of potassium ion batteries.
Smart Images

Figure CN118943292A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a positive electrode sheet and a preparation method thereof, and a hybrid ion battery. Background Art
[0002] Potassium and lithium have similar standard redox potentials, but potassium has abundant reserves in the earth's crust (1.5wt%), which leads to low cost of potassium ion batteries. At the same time, potassium ions have fast ion transport kinetics in the electrolyte, which makes potassium ion batteries have excellent prospects, and thus potassium ion batteries have been rapidly developed. Currently, the positive electrode materials that can be used in potassium ion batteries are mainly divided into polyanions, Prussian blue, organic positive electrode materials and layered transition metal oxide positive electrode materials. Layered transition metal oxides (A x MO2, A=K, M=V, Mn, Fe, Ni, Cr, Co, etc. and their combinations) are widely used due to their stable framework structure, simple synthesis method, high output voltage and high commercial feasibility.
[0003] Current potassium-ion batteries still face significant challenges in terms of energy density and cycle life, including narrow voltage window, electrode dissolution, corrosion, and unexpected byproducts. These fundamental problems can lead to irreversible capacity loss, poor cycle stability, and short circuits, severely limiting the development of potassium-ion batteries. + Effective storage. Therefore, it is necessary to further improve its cycle performance and energy density to meet actual needs. Usually, the means to improve energy density are mainly to increase voltage and capacity. Since the layered oxide of the positive electrode of the potassium ion battery has poor air stability, the surface of the material is easily broken during the cycle, and side reactions occur after contact with the electrolyte, consuming active potassium, which leads to poor cycle performance and further limits its application. For example, CN113675394A discloses a potassium ion battery positive electrode sheet, which includes aluminum foil and an active material layer coated on the aluminum foil. The active material layer includes an active material, a conductive agent and a binder. The molecular formula of the active material is: K x Mn y Cu 1-y-z Sb z O2(KMCSO), x, y, and z are the atomic numbers respectively. Since the positive electrode cannot prevent the material from being corroded by air during use, there are certain disadvantages. Summary of the Invention
[0004] In view of this, the present invention provides a positive electrode sheet, a preparation method thereof, and a hybrid ion battery. The positive electrode sheet can effectively avoid being corroded by air and has the characteristics of high energy density and good cycle performance.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: In a first aspect, the present invention provides a positive electrode sheet, which includes: a positive electrode current collector; a first active material layer disposed on at least one surface in the thickness direction of the positive electrode current collector; the first active material layer includes a first active material, a first conductive agent, and a binder, and the first active material is a potassium-containing active material; a second active material layer disposed on the surface of the first active material layer away from the positive electrode current collector; the second active material layer includes a second active material, a second conductive agent, and a polymer, and the second active material is a lithium-containing active material.
[0006] In an embodiment of the present invention, the polymer includes at least one of polyvinyl alcohol and polyvinylpyrrolidone.
[0007] In an embodiment of the present invention, the chemical general formula of the first active material is KNi w Fe v Mn m O2, where 0 < w ≤ 0.4, 0 < v ≤ 0.6, 0 < m ≤ 0.6, and w + v + m = 1.
[0008] In an embodiment of the present invention, the chemical general formula of the second active material is LiNi x Co y Mn z O2, where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1.
[0009] Preferably, the molar ratio of the first active material to the second active material is (1 to 11):1.
[0010] Preferably, the molar ratio of the second active material to the polymer is (200 to 1250):1.
[0011] Preferably, the mass ratio of the first active material, the first conductive agent, and the binder in the first active material layer is (5 to 10):1:(0.05 to 0.07).
[0012] Preferably, the mass ratio of the second active material, the second conductive agent, and the polymer in the second active material layer is (4 to 8):1:(5 to 20).
[0013] Preferably, the thickness of the first active material layer is 0.1 to 2 mm.
[0014] Preferably, the thickness of the second active material layer is 0.1 to 2 mm.
[0015] In an embodiment of the present invention, a first projection of the first active material layer in the thickness direction of the positive electrode current collector coincides with a second projection of the second active material layer in the thickness direction of the positive electrode current collector, and the area of the first projection is equal to the area of the second projection.
[0016] In an embodiment of the present invention, the first conductive agent and the second conductive agent independently include at least one of conductive carbon black, acetylene black, graphene, conductive graphite, conductive carbon tubes, and conductive carbon fibers.
[0017] In an embodiment of the present invention, the binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, and sodium carboxymethyl cellulose.
[0018] In a second aspect, the present invention provides a method for preparing the above-mentioned positive electrode sheet, comprising the following steps: S1, uniformly mixing a first active material, a first conductive agent, a binder, and a first solvent to obtain slurry A; The second active material, the second conductive agent, and the second solvent are mixed uniformly to obtain slurry B1; the polymer and the third solvent are mixed, heated and stirred to obtain a polymer solution; the slurry B1 and the polymer solution are mixed uniformly to obtain slurry B2; S2, coating the slurry A on the surface of the positive electrode current collector, and performing a first drying to obtain a pole piece composited with the first active material layer; The slurry B2 is coated on the surface of the electrode sheet composited with the first active material layer, and then subjected to a second drying, roller pressing, and a third drying to obtain a positive electrode sheet.
[0019] Preferably, the temperature of the first drying is 80-120° C., and the time of the first drying is 1-3 hours.
[0020] Preferably, the temperature of the second drying is 80-120° C., and the time of the second drying is 1-3 hours.
[0021] Preferably, the temperature of the third drying is 80-120° C., and the time of the third drying is 20-30 hours.
[0022] In a third aspect, the present invention provides a hybrid ion battery, which comprises the above-mentioned positive electrode sheet and / or the positive electrode sheet prepared by the above-mentioned preparation method.
[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) The positive electrode sheet of the present invention is provided with a second active material layer including a lithium-containing active material and a polymer on the surface of the potassium-containing active material layer. Among them, due to the presence of the polymer, on the one hand, the potassium-containing positive electrode active material can be prevented from being corroded by air, thereby preventing capacity loss. On the other hand, it can also effectively prevent the electrolyte solvent from contacting the broken positive electrode during the cycle, thereby avoiding the occurrence of side reactions and improving the cycle performance. At the same time, due to the presence of the lithium-containing active material, the lithium and potassium ions produce a synergistic effect, which can improve the cycle performance while also increasing the energy density. Therefore, the positive electrode sheet of the present invention effectively improves the problem that traditional potassium ion battery materials are easily corroded by air, thereby losing active potassium, and having poor capacity and cycle performance, and has the characteristics of high energy density and good cycle performance.
[0024] (2) Compared with other methods that dope lithium at the material level or perform multi-step blending during the homogenization or coating process, the preparation method of the present invention simplifies the coating process and improves manufacturability by mixing the polymer and lithium-containing active material during the homogenization process. The preparation method is simpler and more efficient. At the same time, since the polymer acts as a binder, no additional binder is required in the second active material layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the structure of the positive electrode sheet of the present invention, wherein 1 represents the current collector, 2 represents the first active material layer, and 3 represents the second active material layer. DETAILED DESCRIPTION
[0026] The present invention discloses a positive electrode sheet, a method for preparing the same, and a hybrid ion battery. Those skilled in the art can refer to the contents herein and appropriately modify the process parameters to achieve the desired results. It is particularly important to note that all similar substitutions and modifications obvious to those skilled in the art are considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments. It is obvious that relevant personnel can modify or appropriately alter and combine the methods and applications described herein without departing from the content, spirit, and scope of the present invention to implement and apply the technology of the present invention.
[0027] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes and do not indicate or imply relative importance.
[0028] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms can mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A can include a single element or multiple elements. Item B can include a single element or multiple elements. Item C can include a single element or multiple elements.
[0029] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.
[0030] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0031] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0032] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0033] Specifically, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a positive electrode sheet, comprising: positive electrode current collector; a first active material layer, the first active material layer being disposed on at least one surface of the positive electrode current collector in a thickness direction; the first active material layer comprising a first active material, a first conductive agent, and a binder, wherein the first active material is a potassium-containing active material; The second active material layer is arranged on the surface of the first active material layer away from the positive electrode current collector; the second active material layer includes a second active material, a second conductive agent and a polymer, and the second active material is a lithium-containing active material.
[0034] In an embodiment of the present invention, the polymer includes at least one of polyvinyl alcohol (PVA) and polyvinyl pyrrolidone (PVP).
[0035] Preferably, the molecular weight of the polymer is from 10,000 to 2,000,000. Exemplarily, the molecular weight of the polymer is any value among 10,000, 50,000, 75,000, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,500,000, 2,000,000 or any value within the range formed by any two of the above values.
[0036] In an embodiment of the present invention, the chemical general formula of the first active material is KNi w Fe v Mn m O2, where 0 < w ≤ 0.4, 0 < v ≤ 0.6, 0 < m ≤ 0.6, and w + v + m = 1. Exemplarily, the first active material includes, but is not limited to, KNi 0.33 Fe 0.33 Mn 0.33 O2, KNi 0.3 Fe 0.3 Mn 0.4 O2, KNi 0.2 Fe 0.6 Mn 0.2 O2, KNi 0.1 Fe 0.6 Mn 0.3 O2, KNi 0.4 Fe 0.1 Mn 0.5 O2, KNi 0.1 Fe 0.3 Mn 0.6 O2, and so on.
[0037] In an embodiment of the present invention, the chemical general formula of the second active material is LiNi x Co y Mn z O2, where 0 < x < 1,0.5 Co 0.3 Mn 0.2 O2 and so on.
[0038] Preferably, the molar ratio of the first active substance to the second active substance is (1-11):1. Exemplarily, the molar ratio of the first active substance to the second active substance is any value among 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, and 11:1, or any value within a range consisting of any two of the above values.
[0039] Preferably, the molar ratio of the second active substance to the polymer is (200-1250):1. Exemplarily, the molar ratio of the second active substance to the polymer is any value among 200:1, 250:1, 300:1, 400:1, 450:1, 500:1, 600:1, 700:1, 750:1, 800:1, 900:1, 1000:1, 1100:1, 1200:1, and 1250:1, or any value within a range consisting of any two of the foregoing values.
[0040] Preferably, the mass ratio of the first active material, the first conductive agent, and the binder in the first active material layer is (5-10):1:(0.05-0.07). Exemplarily, the mass ratio of the first active material, the first conductive agent, and the binder in the first active material layer is any of 9.8:1:0.06, 5:1:0.06, 5.3:1:0.06, 5:1:0.07, and 10:1:0.05, or any value within a range consisting of any two of the above values.
[0041] Preferably, the mass ratio of the second active material, the second conductive agent, and the polymer in the second active material layer is (4-8):1:(5-20). Exemplarily, the mass ratio of the second active material, the second conductive agent, and the polymer in the second active material layer is any one of 4.8:1:20, 4.9:1:9.4, 4.7:1:5.5, 6.8:1:6, 7.2:1:5, 6.7:1:20, 4:1:20, and 8:1:5, or any value within a range consisting of any two of the above values.
[0042] Preferably, the thickness of the first active material layer is 0.1 to 2 mm. Exemplarily, the thickness of the first active material layer is any value selected from 0.1 mm, 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, and 2 mm, or any value within a range consisting of any two of the aforementioned values.
[0043] Preferably, the thickness of the second active material layer is 0.1 to 2 mm. Exemplarily, the thickness of the second active material layer is any value selected from 0.1 mm, 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, and 2 mm, or any value within a range consisting of any two of the aforementioned values.
[0044] In an embodiment of the present invention, a first projection of the first active material layer in the thickness direction of the positive electrode current collector coincides with a second projection of the second active material layer in the thickness direction of the positive electrode current collector, and the area of the first projection is equal to the area of the second projection.
[0045] In an embodiment of the present invention, the first conductive agent and the second conductive agent independently include at least one of conductive carbon black, acetylene black, graphene, conductive graphite, conductive carbon tubes, and conductive carbon fibers.
[0046] In an embodiment of the present invention, the binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, and sodium carboxymethyl cellulose.
[0047] In a second aspect, the present invention provides a method for preparing the above-mentioned positive electrode sheet, comprising the following steps: S1, uniformly mixing a first active material, a first conductive agent, a binder, and a first solvent to obtain slurry A; The second active material, the second conductive agent, and the second solvent are mixed uniformly to obtain slurry B1; the polymer and the third solvent are mixed, heated and stirred to obtain a polymer solution; the slurry B1 and the polymer solution are mixed uniformly to obtain slurry B2; S2, coating the slurry A on the surface of the positive electrode current collector, and performing a first drying to obtain a pole piece composited with the first active material layer; The slurry B2 is coated on the surface of the electrode sheet composited with the first active material layer, and then subjected to a second drying, roller pressing, and a third drying to obtain a positive electrode sheet.
[0048] In an embodiment of the present invention, the first solvent and the second solvent are independently organic solvents, such as N-methylpyrrolidone (NMP).
[0049] In an embodiment of the present invention, the third solvent is water.
[0050] In the embodiment of the present invention, the solid contents of slurry A and slurry B1 are both conventional solid contents, for example, 40% to 80%, which is not specifically limited in the present invention.
[0051] In an embodiment of the present invention, the mass-to-volume ratio of the polymer to the third solvent is (1-5):100, measured in g / mL. Exemplarily, the mass-to-volume ratio of the polymer to the third solvent is any value selected from 1:100, 1:50, 3:100, 1:25, and 1:20, or any value within a range consisting of any two of the aforementioned values.
[0052] Preferably, the heating and stirring in step S1 is performed at a temperature of 80-98° C. for 1-2 hours. Heating and stirring are conventional techniques and are not specifically limited in the present invention.
[0053] Preferably, the slurry B1 and the polymer solution are mixed uniformly as follows: after the polymer solution is cooled to 40-50° C., the slurry B1 is added dropwise to the slurry B1 and stirred uniformly.
[0054] Preferably, the temperature of the first drying is 80-120°C, and the time of the first drying is 1-3 hours. Exemplarily, the temperature of the first drying is any one of 80°C, 90°C, 100°C, 110°C, and 120°C, or any value within the range consisting of any two of the above values, and the time of the first drying is any one of 1 hour, 1.5 hours, 2 hours, 2.5 hours, and 3 hours, or any value within the range consisting of any two of the above values.
[0055] Preferably, the second drying temperature is 80-120°C, and the second drying time is 1-3 hours. Exemplarily, the second drying temperature is any one of 80°C, 90°C, 100°C, 110°C, and 120°C, or any value within the range consisting of any two of the above values, and the second drying time is any one of 1 hour, 1.5 hours, 2 hours, 2.5 hours, and 3 hours, or any value within the range consisting of any two of the above values.
[0056] Preferably, the temperature of the third drying is 80-120°C, and the time of the third drying is 20-30 hours. Exemplarily, the temperature of the third drying is any one of 80°C, 90°C, 100°C, 110°C, and 120°C, or any value within the range consisting of any two of the above values, and the time of the third drying is any one of 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours, and 30 hours, or any value within the range consisting of any two of the above values.
[0057] In a third aspect, the present invention provides a hybrid ion battery, which comprises the above-mentioned positive electrode sheet and / or the positive electrode sheet prepared by the above-mentioned preparation method.
[0058] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.
[0059] This application does not have any special restrictions on the negative electrode sheet, separator, and electrolyte in the battery. Those skilled in the art can choose according to actual needs as long as the purpose of this application can be achieved.
[0060] The reagents, instruments and materials used in the present invention can be obtained through commercial channels.
[0061] The present invention will be further described below in conjunction with the embodiments: Example 1: (1) 11.72g of active material (KNi 0.33 Fe 0.33 Mn 0.33 O2, 0.09 mol), 1.2 g of conductive agent carbon black (Super-P) and 0.07 g of binder polyvinylidene fluoride (PVDF) were uniformly dispersed in solvent N-methylpyrrolidone (NMP) and mixed to prepare slurry A.
[0062] Among them, in slurry A, the active material (KNi 0.33 Fe 0.33 Mn 0.33 O2), the mass ratio of conductive agent and binder is 9.8:1:0.06.
[0063] (2) 0.72g active material (LiNi 0.33 Co 0.33 Mn 0.33 O2, 0.008 mol), 0.15 g of conductive agent carbon black (Super-P) were uniformly dispersed in solvent N-methylpyrrolidone (NMP) and mixed to prepare slurry B1; 3 g of PVA (0.00004 mol) was dissolved in 100 mL of deionized water, stirred at 98 ° C for 2 h until clear, cooled to 45 ° C, and slurry B1 was added dropwise with continuous stirring, and stirring was continued for 15 min to obtain slurry B2.
[0064] Among them, in slurry B2, the active material (LiNi 0.33 Co 0.33 Mn 0.33 O2), conductive agent, and PVA in a mass ratio of 4.8:1:20; Active material (KNi 0.33 Fe 0.33 Mn 0.33 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 O2) with a molar ratio of 11:1; Active material (LiNi 0.33 Co 0.33 Mn 0.33The molar ratio of O2) to PVA is 200:1.
[0065] (3) Slurry A was evenly coated on the aluminum foil current collector and the coating was dried at a temperature of 100°C for 2 h. The coating thickness of slurry A was 0.1 mm.
[0066] (4) Slurry B2 is evenly coated on the coating obtained in step (3), and the coating is dried at a temperature of 100°C for 2 hours. The coating thickness of slurry B2 is 0.1 mm. After rolling the coating, a composite electrode is obtained, which is then baked in a vacuum drying oven at 80°C for 24 hours to obtain a positive electrode with a structure as shown below. Figure 1 shown.
[0067] (5) Preparation of hybrid ion batteries: The positive electrode sheet was cut into 12 mm circular pieces using a cutting machine. A CR2032 button-type battery was assembled in a high-purity argon-filled glove box using a 14 mm diameter, 0.2 mm thick potassium metal sheet as the negative electrode, a 0.1 mol / L potassium perchlorate / ethylene carbonate / dimethyl carbonate solution (ethylene carbonate:dimethyl carbonate volume ratio of 1:1) as the electrolyte, and a 16 mm diameter Whatman GF / F glass fiber as the separator.
[0068] Example 2: The only difference between this embodiment and embodiment 1 is that the active material of slurry B1 (LiNi 0.33 Co 0.33 Mn 0.33 O2) was added in an amount of 1.58 g (0.018 mol), and the amount of conductive agent carbon black (Super-P) was added in an amount of 0.32 g; Among them, in slurry B2, the active material (LiNi 0.33 Co 0.33 Mn 0.33 O2), conductive agent, and PVA in a mass ratio of 4.9:1:9.4; Active material (KNi 0.33 Fe 0.33 Mn 0.33 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 O2) with a molar ratio of 5:1; Active material (LiNi 0.33 Co 0.33 Mn 0.33 The molar ratio of O2) to PVA is 450:1.
[0069] Example 3: The only difference between this embodiment and embodiment 1 is that the active material of slurry B1 (LiNi 0.33 Co 0.33 Mn 0.33 O2) was added in an amount of 2.6 g (0.03 mol), and the conductive agent carbon black (Super-P) was added in an amount of 0.55 g; Among them, in slurry B2, the active material (LiNi 0.33 Co 0.33 Mn 0.33 O2), conductive agent, and PVA in a mass ratio of 4.7:1:5.5; Active material (KNi 0.33 Fe 0.33 Mn 0.33 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 O2) with a molar ratio of 3:1; Active material (LiNi 0.33 Co 0.33 Mn 0.33 The molar ratio of O2) to PVA is 750:1.
[0070] Example 4: The only difference between this embodiment and embodiment 1 is that the active material of slurry B1 (LiNi 0.33 Co 0.33 Mn 0.33 O2) was added in an amount of 3.4 g (0.04 mol), and the conductive agent carbon black (Super-P) was added in an amount of 0.5 g; Among them, in slurry B2, the active material (LiNi 0.33 Co 0.33 Mn 0.33 O2), conductive agent, and PVA in a mass ratio of 6.8:1:6; Active material (KNi 0.33 Fe 0.33 Mn 0.33 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 O2) with a molar ratio of 2.3:1; Active material (LiNi 0.33 Co 0.33 Mn 0.33 The molar ratio of O2) to PVA is 1000:1.
[0071] Example 5: The only difference between this embodiment and embodiment 1 is that the active material of slurry B1 (LiNi 0.33Co 0.33 Mn 0.33 O2) was added in an amount of 4.3 g (0.05 mol), and the conductive agent carbon black (Super-P) was added in an amount of 0.6 g; Among them, in slurry B2, the active material (LiNi 0.33 Co 0.33 Mn 0.33 O2), conductive agent, and PVA in a mass ratio of 7.2:1:5; Active material (KNi 0.33 Fe 0.33 Mn 0.33 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 O2) with a molar ratio of 1.8:1; Active material (LiNi 0.33 Co 0.33 Mn 0.33 The molar ratio of O2) to PVA is 1250:1.
[0072] Example 6: The only difference between this embodiment and embodiment 1 is that the active material of slurry B1 is LiNi 0.8 Co 0.1 Mn 0.1 O2, the amount of which is 1 g (0.02 mol); Among them, in slurry B2, the active material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive agent, and PVA in a mass ratio of 6.7:1:20; Active material (KNi 0.33 Fe 0.33 Mn 0.33 O2) and active material (LiNi 0.8 Co 0.1 Mn 0.1 O2) with a molar ratio of 4.5:1; Active material (LiNi 0.8 Co 0.1 Mn 0.1 The molar ratio of O2) to PVA is 500:1.
[0073] Example 7: The only difference between this embodiment and embodiment 1 is that the active material of slurry A is KNi 0.3 Fe 0.3 Mn 0.4 O2, the amount of which added is 5.87 g (0.05 mol); In slurry A, the active material (KNi 0.3 Fe 0.3 Mn 0.4 O2), the mass ratio of conductive agent and binder is 5:1:0.06; Active material (KNi 0.3 Fe 0.3 Mn 0.4 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 The molar ratio of O2) is 6.3:1.
[0074] Example 8: The only difference between this embodiment and embodiment 1 is that the active material of slurry A is KNi 0.2 Fe 0.6 Mn 0.2 O2, the amount of which is added is 6.4 g (0.05 mol); In slurry A, the active material (KNi 0.2 Fe 0.6 Mn 0.2 O2), the mass ratio of conductive agent and binder is 5.3:1:0.06; Active material (KNi 0.2 Fe 0.6 Mn 0.2 O2) and active material (LiNi 0.33 Co 0.33 Mn 0.33 The molar ratio of O2) is 6.3:1.
[0075] Example 9: The only difference between this embodiment and embodiment 1 is that the polymer PVA in step (2) is replaced by polyvinylpyrrolidone (PVP).
[0076] Comparative Example 1: (1) 7.5g active substance (KNi 0.33 Fe 0.33 Mn 0.33 O2), 1.5g of conductive agent carbon black (Super-P) and 0.07g of binder polyvinylidene fluoride (PVDF) were uniformly dispersed in solvent N-methylpyrrolidone (NMP) and mixed to prepare slurry A.
[0077] (2) Slurry A was evenly applied to the coating obtained in step (2), and the coating was dried at a temperature of 80°C for 2 hours. The coating was rolled to obtain a composite electrode, which was then baked in a vacuum drying oven at 80°C for 24 hours to obtain a positive electrode.
[0078] (3) Preparation of hybrid ion batteries: The positive electrode sheet was cut into 12 mm circular pieces using a cutting machine. A CR2032 button-type battery was assembled in a high-purity argon-filled glove box using a 14 mm diameter, 0.2 mm thick potassium metal sheet as the negative electrode, a 0.1 mol / L potassium perchlorate / ethylene carbonate / dimethyl carbonate solution (ethylene carbonate:dimethyl carbonate volume ratio of 1:1) as the electrolyte, and a 16 mm diameter Whatman GF / F glass fiber as the separator.
[0079] Performance Testing Use constant current charge and discharge mode to conduct charge and discharge tests at a current density of 0.1C. Test items include: (1) 0.1C first cycle discharge capacity: First cycle discharge capacity test: The hybrid ion battery was placed at 25°C for 30 minutes, charged at 0.1C constant current to 4V, then charged at constant voltage to 0.05C, and then discharged at 0.1C constant current to 1.5V. The discharge capacity at this time was recorded as the first cycle discharge capacity.
[0080] (2) 1 C 100-cycle capacity retention rate: Cycle performance test: The hybrid ion battery was placed at 25°C for 30 minutes, charged at a constant current of 1C to 4V, then charged at a constant voltage to 0.05C, and then discharged at a constant current of 1C to 1.5V. The discharge capacity at this time was recorded as the discharge capacity of the first cycle. The battery was placed at rest for 10 minutes, and the capacity of the hybrid ion battery at the 100th cycle was recorded.
[0081] The test results are shown in Table 1 below.
[0082] Table 1 As can be seen from the data in Table 1, the positive electrode sheets prepared in Examples 1-9 of the present invention have better discharge capacity and capacity retention during the charge and discharge process compared to Comparative Example 1. Among them, the positive electrode sheet prepared in Example 5 has better electrical performance.
[0083] In summary, the positive electrode sheet prepared by the present invention can significantly improve the capacity utilization and cycle performance of traditional potassium ion batteries.
[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises: Positive electrode current collector; a first active material layer, the first active material layer being disposed on at least one surface of the positive electrode current collector in a thickness direction; the first active material layer comprising a first active material, a first conductive agent and a binder, the first active material being an active material containing potassium; The second active material layer is arranged on the surface of the first active material layer away from the positive electrode current collector; the second active material layer comprises a second active material, a second conductive agent and a polymer, and the second active material is a lithium-containing active material.
2. The positive electrode sheet according to claim 1, characterized in that: The polymer includes at least one of polyvinyl alcohol and polyvinyl pyrrolidone.
3. The positive electrode sheet according to claim 1, characterized in that: The chemical general formula of the first active substance is KNi w Fe v Mn m O2, where 0 < w ≤ 0.4, 0 < v ≤ 0.6, 0 < m ≤ 0.6, and w + v + m = 1; Preferably, the chemical general formula of the second active substance is LiNi x Co y Mn z O2, where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1.
4. The positive electrode sheet according to claim 1, characterized in that: The molar ratio of the first active substance to the second active substance is (1-11):1; Preferably, the molar ratio of the second active substance to the polymer is (200-1250):
1.
5. The positive electrode sheet according to claim 1, characterized in that: The mass ratio of the first active material, the first conductive agent, and the binder in the first active material layer is (5-10):1:(0.05-0.07); Preferably, the mass ratio of the second active material, the second conductive agent, and the polymer in the second active material layer is (4-8):1:(5-20).
6. The positive electrode sheet according to claim 1, characterized in that: The thickness of the first active material layer is 0.1 to 2 mm; Preferably, the thickness of the second active material layer is 0.1 to 2 mm; Preferably, a first projection of the first active material layer in the thickness direction of the positive electrode current collector coincides with a second projection of the second active material layer in the thickness direction of the positive electrode current collector, and an area of the first projection is equal to an area of the second projection.
7. The positive electrode sheet according to claim 1, characterized in that: The first conductive agent and the second conductive agent independently include at least one of conductive carbon black, acetylene black, graphene, conductive graphite, conductive carbon tube, and conductive carbon fiber; Preferably, the binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, and sodium carboxymethyl cellulose.
8. The method for preparing the positive electrode sheet according to any one of claims 1 to 7, characterized in that: The steps include: S1, mixing a first active material, a first conductive agent, a binder, and a first solvent uniformly to obtain slurry A; The second active material, the second conductive agent and the second solvent are mixed uniformly to obtain slurry B1; the polymer and the third solvent are mixed, and heated and stirred to obtain a polymer solution; the slurry B1 and the polymer solution are mixed uniformly to obtain slurry B2; S2, coating the slurry A on the surface of the positive electrode current collector, and performing a first drying to obtain a pole piece composited with a first active material layer; The slurry B2 is coated on the surface of the electrode sheet composited with the first active material layer, and the positive electrode sheet is obtained after a second drying, a rolling press, and a third drying.
9. The preparation method according to claim 8, characterized in that: The temperature of the first drying is 80 to 120° C., and the time of the first drying is 1 to 3 hours; Preferably, the temperature of the second drying is 80-120° C., and the time of the second drying is 1-3 hours; Preferably, the temperature of the third drying is 80-120° C., and the time of the third drying is 20-30 hours.
10. A hybrid ion battery, characterized in that: The hybrid ion battery comprises the positive electrode sheet according to any one of claims 1 to 7, and / or the positive electrode sheet prepared by the preparation method according to any one of claims 8 to 9.
Citation Information
Patent Citations
Potassium ion battery positive electrode material, preparation method and potassium ion battery
CN113675394A
Preparation method of KLi3Fe(C2O4)3, battery positive electrode active material, battery and electric equipment
CN111349000A
Potassium ion-doped carbon-coated lithium-rich ternary positive electrode material as well as preparation method and application thereof
CN112786875A
Lithium-potassium mixed ion battery and preparation method thereof
CN115966773A
Lithium-sodium-potassium mixed type positive electrode active material as well as preparation method and application thereof
CN116190641A
Cited By
Positive plate, preparation method thereof and battery
CN120674454A