Super flash memory and manufacturing method thereof
By inserting a silicon nitride layer between the oxide layer of the floating gate and the HTO oxide layer, the TiN layer is prevented from oxidizing, and the problem that the floating gate is easily oxidized in the high-temperature process is solved, and the erasing performance is improved.
Patent Information
- Application Number
- CN202310538578.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
The floating gate TiN layer of the existing super flash memory is easily oxidized during the high-temperature process, resulting in a high erase voltage and a slow speed, which affects the erase performance of the device.
The third silicon nitride layer is inserted between the second oxide layer of the floating gate and the subsequent HTO oxide layer, and combined with the protective effect of the fifth silicon nitride layer, preventing the TiN layer from being oxidized, thereby improving the structural continuity of the floating gate and Erase performance.
It effectively prevents oxidation of the TiN layer, improves the structural continuity of the floating gate and the erasing performance of the device, reduces the erasing voltage, and improves the erasing rate.
Smart Images

Figure CN118946147A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor integrated circuit, and more particularly to a super flash memory (SF). The present invention also relates to a method for manufacturing a super flash memory. Background Art
[0002] SF2.0 structure flash memory uses horizontal electric field write operation and cutting-edge TiN voltage-free coupling erase operation to greatly improve erase efficiency and reduce operating voltage. The new structure can increase the nested window of erase gate (EG) to floating gate (FG) and better tip control, and is expected to have better endurance performance. The cell area is only 60% of the same generation SF, and the expected cost can be greatly reduced.
[0003] like Figure 1 The figure is a schematic diagram of the structure of the existing super flash memory; the existing super flash memory includes:
[0004] The first gate trench 103 is formed on the top of the source region 102 , and the bottom surface of the first gate trench 103 is lower than the top surface of the semiconductor substrate 101 , and the top surface of the first gate trench 103 is higher than the top surface of the semiconductor substrate 101 .
[0005] Typically, the semiconductor substrate 101 includes a silicon substrate.
[0006] The source region 102 is formed in a surface region of the semiconductor substrate 101 at the bottom of the first gate trench 103 .
[0007] Usually, perpendicular to Figure 1 In the paper direction corresponding to the cross section, the source regions 102 of the storage cells of different super flash memories are connected together to form a source region line (SL).
[0008] A floating gate 105 and a control gate 107 are formed in the first gate trench 103 .
[0009] Usually, the control gate 107 is made of tungsten. The control gate 107 is in direct contact with the source region 102 at the bottom.
[0010] An oxide layer 104 is formed between the first side surface of the floating gate 105 and the side surface and bottom surface of the first gate trench 103. The oxide layer 104 is a HTO oxide layer.
[0011] An oxide layer 106 is formed between the second side of the floating gate 105 and the side of the control gate 107. The oxide layer 106 is usually formed by stacking an atomic layer deposition (ALD) oxide layer and a high temperature oxide (HTO) oxide layer, wherein the ALD oxide layer is an oxide layer formed by the ALD process, and the HTO oxide layer is an oxide layer formed by the HTO process.
[0012] The floating gate 105 is made of a TiN layer; the top of the floating gate 105 is higher than the top surface of the control gate 107 .
[0013] Two word line gates 108 are symmetrically arranged on the semiconductor substrate 101 at two sides of the first gate trench 103 , and a first gate dielectric layer (not shown) is provided between the word line gates 108 and the semiconductor substrate 101 .
[0014] A dielectric layer 109 is isolated between the side surface of the first gate trench 103 and the second side surface of the word line gate 108 , and a first inter-gate dielectric layer is formed by stacking the dielectric layer 109 and the oxide layer 104 .
[0015] An erase gate 113 is formed on the top of the first gate trench 103 and the area covered by the erase gate 113 is larger than the formation area of the first gate trench 103; a second inter-gate dielectric layer 112 is isolated between the erase gate 113 and the first inter-gate dielectric layer, the floating gate 105 and the oxide layer 106 at the bottom.
[0016] Usually, the dielectric layer 109 and the second inter-gate dielectric layer 112 are both oxide layers. Figure 1 The images corresponding to the dielectric layer 109 , the second inter-gate dielectric layer 112 , the oxide layer 104 , and the oxide layer 106 are all filled with the same dots.
[0017] The drain region 111 is self-aligned and formed in the surface area of the semiconductor substrate 101 on the first side of the word line gate 108. Usually, a sidewall (not shown) is also formed on the first side of the word line gate 108, and the drain region 111 is self-aligned with the sidewall of the first side of the word line gate 108. A lightly doped drain region (LDD) 110 is also formed on one side of the drain region 111, and the lightly doped drain region 110 is self-aligned with the first side of the word line gate 108.
[0018] Typically, the word line gate 108 is a polysilicon gate or a metal gate; the erase gate 113 is a polysilicon gate or a metal gate.
[0019] like FIG. 2A to FIG. 2BFIG. 1 is a schematic diagram of a device structure in each sub-step of forming a floating gate in an existing method for manufacturing a super flash memory; the existing method for manufacturing a super flash memory comprises the following steps:
[0020] Step 1: Figure 1 As shown, a first gate trench 103 is formed in the formation region of the floating gate 105 and the control gate 107, the first gate trench 103 is located at the top of the formation region of the source region 102, the bottom surface of the first gate trench 103 is lower than the top surface of the semiconductor substrate 101, and the top surface of the first gate trench 103 is higher than the top surface of the semiconductor substrate 101.
[0021] Step 2: forming a source region 102 in the surface area of the semiconductor substrate 101 at the bottom of the first gate trench 103 .
[0022] Step 3: forming the floating gate 105, including the following steps:
[0023] Step 31: Figure 2A As shown, an oxide layer 104 a is formed on the side and bottom surfaces of the first gate trench 103 .
[0024] In the existing method, the oxide layer 104a is formed by using a HTO oxidation process.
[0025] Step 32: Figure 2A As shown, a TiN layer 105a of the floating gate 105 is formed on the surface of the oxide layer 104a.
[0026] Step 33: Figure 2A As shown, an oxide layer 106a is formed on the surface of the TiN layer 105a.
[0027] In the existing method, the oxide layer 106a is formed by using a HTO oxidation process.
[0028] Step 34: Figure 2B As shown, the oxide layer 106a, the TiN layer 105a and the oxide layer 104a are completely etched (blank etch) so that the oxide layer 106, the TiN layer and the oxide layer 104 are only retained on the side of the first gate trench 103 and form a sidewall structure. The oxide layer 106a, the TiN layer 105a and the oxide layer 104a on the bottom surface of the first gate trench 103 outside the sidewall structure and outside the first gate trench 103 are all removed; the floating gate 105 is formed by the retained TiN layer. Figure 2B In the figure, the etched oxide layer, the TiN layer and the oxide layer are represented by reference numerals 106, 105 and 104 respectively.
[0029] like FIG. 3A to FIG. 3B , which is a schematic diagram of the device structure in each sub-step of forming a floating gate in an existing improved method for manufacturing a super flash memory; FIG. 3A to FIG. 3B The manufacturing method of the existing improved super flash memory and Figure 2A-2B The difference between the corresponding existing improved super flash memory manufacturing method is as follows:
[0030] In step 33 of step three, after forming the oxide layer 106a, a step of forming a silicon nitride layer 114a is also included. The nitride layer 114a serves as a coupling silicon nitride layer (coupling SiN) and is usually grown by an ALD process.
[0031] In this way, in step 34, the silicon nitride layer 114a will be etched first, and then the oxide layer 106a, the TiN layer 105a and the oxide layer 104a will be fully etched in turn, and then the silicon nitride layer 114, the oxide layer 106, the TiN layer and the oxide layer 104 will be formed after etching, which will only remain on the side of the first gate trench 103.
[0032] Since the TiN layer of the floating gate 105 has oxygen elements around it, it is easily oxidized during the high-temperature process, which can easily make the entire TiN layer serving as the floating gate 105 discontinuous, which will have an adverse effect on the erase operation, such as a high erase voltage and a slow erase rate.
[0033] FIG. 3A to FIG. 3B In the corresponding existing improved super flash memory manufacturing method, the silicon nitride layer 114 is added to protect the TiN layer to a certain extent. However, the results of energy dispersive spectrometer (EDS) and transmission electron microscope (TEM) show that under the influence of the surrounding environment and process, the top area of the TiN layer of the floating gate 105 is still easily oxidized, resulting in a high erase voltage and a slow speed. Figure 3B The element content of each region of the floating gate 105 is analyzed as shown below:
[0034] It is found that the oxygen content in the top region of the TiN layer of the floating gate 105 is higher than that in other regions, and the Ti / N ratio is higher than that in the bottom and middle regions. The top region of the TiN layer of the floating gate 105 is the erasing region, and oxidation of the top region can easily have an adverse effect on the erasing performance. Summary of the invention
[0035] The technical problem to be solved by the present invention is to provide a super flash memory, which can improve the structural continuity of the TiN layer of the floating gate and thus improve the erasing performance of the device. To this end, the present invention also provides a method for manufacturing the super flash memory.
[0036] In order to solve the above technical problems, the device unit of the super flash memory provided by the present invention is located in the storage area, and the device unit includes:
[0037] A first gate trench is formed on the top of the source region, and a bottom surface of the first gate trench is lower than a top surface of the semiconductor substrate and a top surface of the first gate trench is higher than a top surface of the semiconductor substrate.
[0038] The source region is formed in a surface region of the semiconductor substrate at a bottom of the first gate trench.
[0039] A first sidewall structure is self-alignedly formed on the side of the first gate trench, and the first sidewall structure is formed by self-aligned etching of a first stacked layer, and the first stacked layer is formed by stacking a first tunneling dielectric layer, a floating gate, and a second oxide layer, the first tunneling dielectric layer is formed on the side and bottom surfaces of the first gate trench, the floating gate is formed on the surface of the first tunneling dielectric layer, and the second oxide layer is formed on the surface of the floating gate.
[0040] The material of the floating gate includes a TiN layer.
[0041] The second side surface of the first sidewall structure is formed by superposition of the second side surface of the second oxide layer and the etched surface of the floating gate and the first tunneling dielectric layer located at the bottom of the second side surface of the second oxide layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the first sidewall structure.
[0042] A second sidewall structure is self-alignedly formed on the second side of the first sidewall structure, the second sidewall structure is formed by self-aligned etching of a second stacked layer, and the second stacked layer is formed by stacking a third silicon nitride layer, a fourth oxide layer and a fifth silicon nitride layer; the third silicon nitride layer is formed on the second side of the first sidewall structure and the bottom surface of the first gate trench, the fourth oxide layer is formed on the surface of the third silicon nitride layer, and the fifth silicon nitride layer is formed on the surface of the fourth oxide layer.
[0043] The second side surface of the second sidewall structure is formed by superimposing the second side surface of the fifth silicon nitride layer and the etched surfaces of the fourth oxide layer and the third silicon nitride layer located at the bottom of the second side surface of the fifth silicon nitride layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the second sidewall structure.
[0044] The second oxide layer is an ALD oxide layer.
[0045] The fourth oxide layer is a HTO oxide layer.
[0046] The third silicon nitride layer serves as a protection layer of the floating gate to prevent the TiN layer of the floating gate from being oxidized.
[0047] A further improvement is that a control gate is filled in the first gate trench between the second side surfaces of the second spacer structure and the control gate is in contact with the source region at the bottom.
[0048] Two word line gates are symmetrically arranged on the semiconductor substrate at two sides of the first gate trench, and a first gate dielectric layer is separated between the word line gates and the semiconductor substrate.
[0049] A sixth dielectric layer is provided between the side surface of the first gate trench and the second side surface of the word line gate.
[0050] An erase gate is formed in the top region of the floating gate, and a second tunnel dielectric layer is spaced between the erase gate and the floating gate.
[0051] A drain region is formed in a self-aligned manner in a surface region of the semiconductor substrate at a first side of the word line gate.
[0052] A further improvement is that the first tunnel dielectric layer is a HTO oxide layer.
[0053] A further improvement is that the third silicon nitride layer is an ALD silicon nitride layer; and the fifth silicon nitride layer is an ALD silicon nitride layer.
[0054] A further improvement is that the thickness of the first tunnel dielectric layer is
[0055] The thickness of the second oxide layer is
[0056] The thickness of the third silicon nitride layer is
[0057] The thickness of the fourth oxide layer is
[0058] The thickness of the fifth silicon nitride layer is
[0059] A further improvement is that the thickness of the TiN layer of the floating gate is
[0060] In order to solve the above technical problems, in the manufacturing method of the super flash memory provided by the present invention, the device unit is located in the storage area, and the steps of forming the device unit include:
[0061] Step 1: forming a first gate trench, wherein the first gate trench is located at the top of the source region formation area, the bottom surface of the first gate trench is lower than the top surface of the semiconductor substrate, and the top surface of the first gate trench is higher than the top surface of the semiconductor substrate.
[0062] Step 2: forming the source region in the surface area of the semiconductor substrate at the bottom of the first gate trench.
[0063] Step 3: forming a first sidewall structure by self-alignment on the side of the first gate trench, including the following steps:
[0064] Step 31, forming a first tunneling dielectric layer on the side and bottom surfaces of the first gate trench, forming a floating gate on the surface of the first tunneling dielectric layer, forming a second oxide layer on the surface of the floating gate, and forming a first stacking layer by stacking the first tunneling dielectric layer, the floating gate and the second oxide layer; the first stacking layer also extends to the surface outside the first gate trench.
[0065] The material of the floating gate includes a TiN layer.
[0066] The second oxide layer is an ALD oxide layer.
[0067] Step 32: sequentially etch the second oxide layer, the floating gate, and the first tunnel dielectric layer to form a first sidewall structure in self-alignment on the side of the first gate trench.
[0068] The second side surface of the first sidewall structure is formed by superposition of the second side surface of the second oxide layer and the etched surface of the floating gate and the first tunneling dielectric layer located at the bottom of the second side surface of the second oxide layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the first sidewall structure.
[0069] Step 4: forming a second sidewall structure by self-alignment on the second side of the first sidewall structure, including the following steps:
[0070] Step 41: Form a third silicon nitride layer on the second side surface of the first spacer structure and the bottom surface of the first gate trench, form a fourth oxide layer on the surface of the third silicon nitride layer, and form a fifth silicon nitride layer on the surface of the fourth oxide layer; and form a second stacked layer by stacking the third silicon nitride layer, the fourth oxide layer, and the fifth silicon nitride layer. The second stacked layer also extends to the top surface of the first spacer structure and the surface outside the first gate trench.
[0071] The fourth oxide layer is a HTO oxide layer.
[0072] The third silicon nitride layer serves as a protection layer of the floating gate to prevent the TiN layer of the floating gate from being oxidized.
[0073] Step 42: sequentially etch the fifth silicon nitride layer, the fourth oxide layer, and the third silicon nitride layer to form the second spacer structure on the second side of the first spacer structure in a self-aligned manner.
[0074] The second side surface of the second sidewall structure is formed by superimposing the second side surface of the fifth silicon nitride layer and the etched surfaces of the fourth oxide layer and the third silicon nitride layer located at the bottom of the second side surface of the fifth silicon nitride layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the second sidewall structure.
[0075] A further improvement is that in step 1, two word line gates are symmetrically arranged on the semiconductor substrate at both sides of the first gate trench, and a first gate dielectric layer is separated between the word line gates and the semiconductor substrate.
[0076] A sixth dielectric layer is provided between the side surface of the first gate trench and the second side surface of the word line gate.
[0077] After step 4 is completed, the method further includes: step 5, filling a control gate in the first gate trench between the second side surfaces of the second spacer structure, wherein the control gate is in contact with the source region at the bottom.
[0078] After step 5 is completed, it also includes:
[0079] An erase gate and a second tunnel dielectric layer located between the erase gate and the floating gate are formed in a top region of the floating gate.
[0080] After the first side of the word line gate is formed, the method further includes:
[0081] A drain region is formed in a self-aligned manner in a surface region of the semiconductor substrate at a first side of the word line gate.
[0082] A further improvement is that the first tunnel dielectric layer is an HTO oxide layer grown by an HTO process.
[0083] A further improvement is that the third silicon nitride layer is an ALD silicon nitride layer formed by an ALD process; and the fifth silicon nitride layer is an ALD silicon nitride layer formed by an ALD process.
[0084] A further improvement is that the thickness of the first tunnel dielectric layer is
[0085] The thickness of the second oxide layer is
[0086] The thickness of the third silicon nitride layer is
[0087] The thickness of the fourth oxide layer is
[0088] The thickness of the fifth silicon nitride layer is
[0089] A further improvement is that the temperature of the HTO process of the first tunnel dielectric layer is 600°C to 900°C.
[0090] A further improvement is that the TiN layer of the floating gate is formed by deposition using a PVD process.
[0091] A further improvement is that the temperature of the PVD process of the TiN layer of the floating gate is 400 degrees Celsius.
[0092] A further improvement is that the thickness of the TiN layer of the floating gate is
[0093] A further improvement is that a non-storage area is also included outside the storage area.
[0094] In step 1, while forming the first gate trench, the method also includes forming a second gate trench in the non-storage area, wherein the second gate trench is located above a field oxide formed on the semiconductor substrate.
[0095] In step 31 , the first stacking layer is also formed on the inner surface of the second gate trench and the surface outside the second gate trench.
[0096] In step 32, before performing the etching process of the first sidewall structure, the process further includes:
[0097] A first mask layer is formed to cover the storage area and open the non-storage area.
[0098] The first stacking layer in the non-storage area is removed by using the first mask layer as a mask.
[0099] The first mask layer is removed by etching.
[0100] A further improvement is that in step 32, the process of etching the TiN layer of the floating gate in the first stacking layer adopts wet etching, and the wet etching solution adopts a mixed cleaning solution of HF, H2O2 and H2O.
[0101] A further improvement is that, in step 42, the etching process for the fifth silicon nitride layer, the fourth oxide layer and the third silicon nitride layer is a dry etching process.
[0102] The present invention inserts a third silicon nitride layer between the second oxide layer on the surface of the floating gate and the fourth oxide layer composed of the subsequent HTO oxide layer. The third silicon nitride layer can serve as a protective layer for the TiN layer of the floating gate, especially in the HTO oxidation process of the fourth oxide layer, to provide protection for the TiN layer to prevent the TiN layer from being oxidized, especially to prevent the top area of the TiN layer from being oxidized. Combined with the protective effect of the fifth silicon nitride layer, the structural continuity of the TiN layer of the floating gate can be improved, thereby improving the erasing performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0103] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0104] Figure 1 It is a schematic diagram of the structure of the existing 38 super flash memory;
[0105] Figure 2A-2B It is a schematic diagram of the device structure in each sub-step of forming a floating gate in the existing super flash memory manufacturing method;
[0106] Figure 3A-3B It is a schematic diagram of the device structure in each sub-step of forming a floating gate in an existing improved method for manufacturing a super flash memory;
[0107] Figure 4 is a schematic diagram of the structure of a super flash memory according to an embodiment of the present invention;
[0108] Figure 5A-5G It is a schematic diagram of the device structure in each sub-step of forming a floating gate in the manufacturing method of a super flash memory according to an embodiment of the present invention. DETAILED DESCRIPTION
[0109] like Figure 4 , which is a schematic diagram of the structure of a super flash memory according to an embodiment of the present invention; the device unit of the super flash memory according to the embodiment of the present invention is located in the storage area 303, and the device unit includes:
[0110] The first gate trench 203 is formed on the top of the source region 202 , and the bottom surface of the first gate trench 203 is lower than the top surface of the semiconductor substrate 201 , and the top surface of the first gate trench 203 is higher than the top surface of the semiconductor substrate 201 .
[0111] The semiconductor substrate 201 includes a silicon substrate.
[0112] The source region 202 is formed in a surface region of the semiconductor substrate 201 at the bottom of the first gate trench 203 .
[0113] A first sidewall structure 301 is formed by self-alignment on the side of the first gate trench 203. The first sidewall structure 301 is formed by self-alignment etching of the first stacking layer 301a. Figure 5B As shown, the first stacked layer 301a is formed by stacking a first tunnel dielectric layer 204a, a floating gate 205a, and a second oxide layer 2061a, wherein the first tunnel dielectric layer 204a is formed on the side and bottom surfaces of the first gate trench 203, the floating gate 205a is formed on the surface of the first tunnel dielectric layer 204a, and the second oxide layer 2061a is formed on the surface of the floating gate 205a. After self-aligned etching, the first tunnel dielectric layer in the first spacer structure 301 is represented by a mark 204, the floating gate is represented by a mark 205, and the second oxide layer is represented by a mark 2061.
[0114] The material of the floating gate 205 includes a TiN layer.
[0115] The second side surface of the first sidewall structure 301 is formed by superimposing the second side surface of the second oxide layer 2061 and the etched surface of the floating gate 205 and the first tunneling dielectric layer 204 located at the bottom of the second side surface of the second oxide layer 2061; the bottom surface of the first gate trench 203 is exposed between the second side surfaces of the first sidewall structure 301.
[0116] A second sidewall spacer 302 is formed by self-alignment on the second side of the first sidewall spacer 301. The second sidewall spacer 302 is formed by self-alignment etching of the second stacking layer 302a. For the structure of the second stacking layer 302a, please refer to Fig. 5F As shown, the second stacked layer 302a is formed by stacking a third silicon nitride layer 2062a, a fourth oxide layer 2063a and a fifth silicon nitride layer 2064a; the third silicon nitride layer 2062a is formed on the second side surface of the first spacer structure 301 and the bottom surface of the first gate trench 203, the fourth oxide layer 2063a is formed on the surface of the third silicon nitride layer 2062a, and the fifth silicon nitride layer 2064a is formed on the surface of the fourth oxide layer 2063a. After self-aligned etching, the third silicon nitride layer in the second spacer structure 302 is represented by a mark 2062, the fourth oxide layer is represented by a mark 2063, and the fifth silicon nitride layer is represented by a mark 2064.
[0117] The second side surface of the second sidewall structure 302 is formed by the second side surface of the fifth silicon nitride layer 2064 and the etched surfaces of the fourth oxide layer 2063 and the third silicon nitride layer 2062 located at the bottom of the second side surface of the fifth silicon nitride layer 2064; the bottom surface of the first gate trench 203 is exposed between the second side surfaces of the second sidewall structure 302.
[0118] The control gate 207 is filled in the first gate trench 203 between the second side surfaces of the second spacer structure 302 , and the control gate 207 is in contact with the source region 202 at the bottom.
[0119] In some embodiments, the control gate 207 is formed of tungsten material.
[0120] The second oxide layer 2061 is an ALD oxide layer.
[0121] The fourth oxide layer 2063 is a HTO oxide layer.
[0122] The third silicon nitride layer 2062 serves as a protection layer of the floating gate 205 to prevent the TiN layer of the floating gate 205 from being oxidized.
[0123] In the embodiment of the present invention, two word line gates 208 are symmetrically arranged on the semiconductor substrate 201 at both sides of the first gate trench 203 , and a first gate dielectric layer (not shown) is separated between the word line gates 208 and the semiconductor substrate 201 .
[0124] A sixth dielectric layer 209 is provided between the side surface of the first gate trench 203 and the second side surface of the word line gate 208 .
[0125] An erase gate 213 is formed at the top region of the floating gate 205, and a second tunnel dielectric layer 212 is spaced between the erase gate 213 and the floating gate 205. When the floating gate 205 is erased, the charges stored in the floating gate 205 pass through the second tunnel dielectric layer 212 and enter the erase gate 213, thereby erasing the floating gate 205.
[0126] In the embodiment of the present invention, the erase gate 213 will simultaneously cover the floating gate 205 on both sides of the first gate trench 203; the width of the erase gate 213 is usually set to be greater than the width of the first gate trench 203. The second tunneling dielectric layer 212 also serves as an inter-gate dielectric layer between the erase gate 213 and the word line gate 208 and the control gate 207 at the bottom.
[0127] In the embodiment of the present invention, the sixth dielectric layer 209, the second tunnel dielectric layer 212, and the first tunnel dielectric layer 204 are all oxide layers. Figure 4 The images corresponding to the sixth dielectric layer 209, the second tunnel dielectric layer 212, the first tunnel dielectric layer 204, the fourth oxide layer 2063 and the second oxide layer 2061 are all filled with the same dots.
[0128] The drain region 211 is self-aligned and formed in the surface region of the semiconductor substrate 201 at the first side of the word line gate 208. In some embodiments, a lightly doped drain region 210 is also formed in the surface region of the semiconductor substrate 201 at the first side of the word line gate 208.
[0129] In some embodiments, the first tunnel dielectric layer 204 is a HTO oxide layer. When programming the floating gate 205, the surface of the channel region covered by the word line gate 208 will be inverted to form a conductive channel to connect the drain region 211 and the source region 202, and hot carriers will be formed near the source region 202 and pass through the first tunnel dielectric layer 204 into the floating gate 205.
[0130] The third silicon nitride layer 2062a is an ALD silicon nitride layer; the fifth silicon nitride layer 2064a is an ALD silicon nitride layer. The TiN layer of the floating gate 205 is formed by deposition using a PVD process.
[0131] The thickness of the first tunnel dielectric layer 204a is
[0132] The thickness of the second oxide layer 2061a is
[0133] The thickness of the third silicon nitride layer 2062a is
[0134] The thickness of the fourth oxide layer 2063a is
[0135] The thickness of the fifth silicon nitride layer 2064a is
[0136] The thickness of the TiN layer of the floating gate 205 is
[0137] In the embodiment of the present invention, a third silicon nitride layer 2062 is inserted between the second oxide layer 2061 on the surface of the floating gate 205 and the fourth oxide layer 2063 composed of the subsequent HTO oxide layer. The third silicon nitride layer 2062 can serve as a protective layer for the TiN layer of the floating gate 205, especially in the HTO oxidation process of the fourth oxide layer 2063, to provide protection for the TiN layer to prevent the TiN layer from being oxidized, especially to prevent the top area of the TiN layer from being oxidized. Combined with the protective effect of the fifth silicon nitride layer 2064, the structural continuity of the TiN layer of the floating gate 205 can be improved, thereby improving the erasing performance of the device.
[0138] like FIG. 5A to FIG. 5G , which is a schematic diagram of the device structure in each sub-step of forming the floating gate 205 in the manufacturing method of the super flash memory according to the embodiment of the present invention; in the manufacturing method of the super flash memory according to the embodiment of the present invention, the device unit is located in the storage area 303, and the steps of forming the device unit include:
[0139] Step 1: Figure 5A As shown, a first gate trench 203 is formed, and the first gate trench 203 is located at the top of the formation area of the source region 202, the bottom surface of the first gate trench 203 is lower than the top surface of the semiconductor substrate 201, and the top surface of the first gate trench 203 is higher than the top surface of the semiconductor substrate 201.
[0140] Figure 5A In FIG. 3 , the storage area 303 and the non-storage area 304 are displayed simultaneously.
[0141] In the embodiments of the present invention, please also refer to Figure 4 As shown, two word line gates 208 are symmetrically arranged on the semiconductor substrate 201 at both sides of the first gate trench 203 , and a first gate dielectric layer is separated between the word line gates 208 and the semiconductor substrate 201 . Figure 5A The word line gate 208 is not shown. Figure 5A Only the area between the word line gates 208 in the storage area 303 is shown.
[0142] A sixth dielectric layer 209 is provided between the side surface of the first gate trench 203 and the second side surface of the word line gate 208 .
[0143] Step 2: forming the source region 202 in the surface area of the semiconductor substrate 201 at the bottom of the first gate trench 203. Figure 4 shown.
[0144] Step 3: forming a first spacer structure 301 by self-alignment on the side of the first gate trench 203, including the following steps:
[0145] Step 31: Figure 5B As shown, a first tunneling dielectric layer 204a is formed on the side and bottom surfaces of the first gate trench 203, a floating gate 205 is formed on the surface of the first tunneling dielectric layer 204a, and a second oxide layer 2061a is formed on the surface of the floating gate 205. The first tunneling dielectric layer 204a, the floating gate 205 and the second oxide layer 2061a are stacked to form a first stacking layer 301a; the first stacking layer 301a also extends to the surface outside the first gate trench 203.
[0146] The material of the floating gate 205 includes a TiN layer.
[0147] The second oxide layer 2061a is an ALD oxide layer.
[0148] In the method of the embodiment of the present invention, the first tunnel dielectric layer 204a is a HTO oxide layer grown by the HTO process. The HTO process growth equipment of the first tunnel dielectric layer 204a is a furnace tube, and the temperature range is 600°C to 900°C.
[0149] The TiN layer of the floating gate 205 is formed by deposition using a PVD process, and the temperature of the PVD process of the TiN layer of the floating gate 205 is 400 degrees Celsius.
[0150] Step 32: Figure 5E As shown, the second oxide layer 2061a, the floating gate 205 and the first tunnel dielectric layer 204a are etched in sequence to form a first spacer structure 301 on the side of the first gate trench 203 in a self-aligned manner.
[0151] The second side surface of the first sidewall structure 301 is formed by superimposing the second side surface of the second oxide layer 2061 and the etched surface of the floating gate 205 and the first tunneling dielectric layer 204 located at the bottom of the second side surface of the second oxide layer 2061; the bottom surface of the first gate trench 203 is exposed between the second side surfaces of the first sidewall structure 301.
[0152] Step 4: Fig. 5F As shown, forming the second spacer structure 302 on the second side of the first spacer structure 301 by self-alignment includes the following steps:
[0153] Step 41: Fig. 5FAs shown, a third silicon nitride layer 2062a is formed on the second side surface of the first spacer structure 301 and the bottom surface of the first gate trench 203, a fourth oxide layer 2063a is formed on the surface of the third silicon nitride layer 2062a, and a fifth silicon nitride layer 2064a is formed on the surface of the fourth oxide layer 2063a; the third silicon nitride layer 2062a, the fourth oxide layer 2063a and the fifth silicon nitride layer 2064a are stacked to form a second stacked layer 302a. The second stacked layer 302a also extends to the top surface of the first spacer structure 301 and the surface outside the first gate trench 203.
[0154] The fourth oxide layer 2063a is a HTO oxide layer.
[0155] The third silicon nitride layer 2062a serves as a protection layer of the floating gate 205 to prevent the TiN layer of the floating gate 205 from being oxidized.
[0156] In the method of the embodiment of the present invention, the third silicon nitride layer 2062a is an ALD silicon nitride layer formed by an ALD process; and the fifth silicon nitride layer 2064a is an ALD silicon nitride layer formed by an ALD process.
[0157] Step 42: Figure 5G As shown, the fifth silicon nitride layer 2064a, the fourth oxide layer 2063a and the third silicon nitride layer 2062a are etched in sequence to form the second spacer structure 302 on the second side of the first spacer structure 301 in a self-aligned manner.
[0158] The second side surface of the second sidewall structure 302 is formed by the second side surface of the fifth silicon nitride layer 2064 and the etched surfaces of the fourth oxide layer 2063 and the third silicon nitride layer 2062 located at the bottom of the second side surface of the fifth silicon nitride layer 2064; the bottom surface of the first gate trench 203 is exposed between the second side surfaces of the second sidewall structure 302.
[0159] Step 5: Figure 4 As shown, a control gate 207 is filled in the first gate trench 203 between the second side surfaces of the second spacer structure 302 , and the control gate 207 is in contact with the source region 202 at the bottom.
[0160] After step 5 is completed, it also includes:
[0161] like Figure 4 As shown, an erase gate 213 and a second tunnel dielectric layer 212 located between the erase gate 213 and the floating gate 205 are formed in the top region of the floating gate 205 .
[0162] After the first side of the word line gate 208 is formed, the method further includes:
[0163] A drain region 211 is formed in a self-aligned manner in a surface region of the semiconductor substrate 201 at a first side of the word line gate 208 .
[0164] In some embodiments, the following parameters can be used:
[0165] The thickness of the first tunnel dielectric layer 204a is
[0166] The thickness of the second oxide layer 2061a is
[0167] The thickness of the third silicon nitride layer 2062a is
[0168] The thickness of the fourth oxide layer 2063a is
[0169] The thickness of the fifth silicon nitride layer 2064a is
[0170] The thickness of the TiN layer of the floating gate 205 is
[0171] In the method of the embodiment of the present invention, a non-storage area 304 is further included outside the storage area 303. The non-storage area 304 includes a source line strap (SL strap) formation area or a word line strap (WL strap) formation area.
[0172] like Figure 5A As shown, in step 1, while forming the first gate trench 203, a second gate trench 203a is formed in the non-storage area 304, and the second gate trench 203a is located above the field oxide 305, and the field oxide 305 is formed on the semiconductor substrate 201.
[0173] like Figure 5B As shown, in step 31, the first stacking layer 301a is also formed on the inner surface of the second gate trench 203a and the outer surface of the second gate trench 203a.
[0174] In step 32, before performing the etching process of the first sidewall structure 301, the process further includes:
[0175] like Figure 5CAs shown, a first mask layer 306 is formed to cover the storage area 303 and to open the non-storage area 304. In some embodiments, the first mask layer 306 is formed using a photoresist pattern, and the photoresist pattern is obtained by a photolithography process, that is, the photoresist is exposed and developed. In the photolithography process of the first mask layer 306, the second oxide layer 2061a serves as a masking layer.
[0176] like Figure 5D As shown, the first stacking layer 301a in the non-storage area 304 is removed by using the first mask layer 306 as a mask.
[0177] like Figure 5E As shown, the first mask layer 306 is removed by etching.
[0178] In some embodiments, in step 32, anisotropic dry etching is used to etch the second oxide layer 2061a; wet etching is used to etch the TiN layer of the floating gate 205 in the first stacking layer 301a, and the wet etching solution is a mixed cleaning solution of HF, H2O2 and H2O.
[0179] In step 42, an anisotropic dry etching process is used to etch the fifth silicon nitride layer 2064a, the fourth oxide layer 2063a and the third silicon nitride layer 2062a, and high-energy plasma is used in the anisotropic dry etching process.
[0180] The present invention has been described in detail above through specific embodiments, but these do not constitute a limitation of the present invention. Without departing from the principle of the present invention, those skilled in the art may also make many variations and improvements, which should also be regarded as the protection scope of the present invention.
Claims
1. A super flash memory, characterized in that: The device unit is located in the storage area, and the device unit includes: A first gate trench is formed at the top of the source region, a bottom surface of the first gate trench is lower than a top surface of the semiconductor substrate, and a top surface of the first gate trench is higher than a top surface of the semiconductor substrate; The source region is formed in the surface region of the semiconductor substrate at the bottom of the first gate trench; A first sidewall structure is self-alignedly formed on the side of the first gate trench, the first sidewall structure is formed by self-aligned etching of a first stacked layer, the first stacked layer is stacked by a first tunneling dielectric layer, a floating gate and a second oxide layer, the first tunneling dielectric layer is formed on the side and bottom surfaces of the first gate trench, the floating gate is formed on the surface of the first tunneling dielectric layer, and the second oxide layer is formed on the surface of the floating gate; The material of the floating gate includes a TiN layer; The second side surface of the first spacer structure is formed by superposition of the second side surface of the second oxide layer and the etched surface of the floating gate and the first tunnel dielectric layer located at the bottom of the second side surface of the second oxide layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the first spacer structure; A second sidewall spacer is self-alignedly formed on the second side of the first sidewall spacer structure, the second sidewall structure is formed by self-aligned etching of a second stacked layer, the second stacked layer is stacked by a third silicon nitride layer, a fourth oxide layer and a fifth silicon nitride layer; the third silicon nitride layer is formed on the second side of the first sidewall spacer structure and the bottom surface of the first gate trench, the fourth oxide layer is formed on the surface of the third silicon nitride layer, and the fifth silicon nitride layer is formed on the surface of the fourth oxide layer; The second side surface of the second spacer structure is formed by stacking the second side surface of the fifth silicon nitride layer and the etched surfaces of the fourth oxide layer and the third silicon nitride layer located at the bottom of the second side surface of the fifth silicon nitride layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the second spacer structure; The second oxide layer is an ALD oxide layer; The fourth oxide layer is a HTO oxide layer; The third silicon nitride layer serves as a protection layer of the floating gate to prevent the TiN layer of the floating gate from being oxidized.
2. The super flash memory as claimed in claim 1, characterized in that: A control gate is filled in the first gate trench between the second side surfaces of the second spacer structure, and the control gate is in contact with the source region at the bottom; Two word line gates are symmetrically arranged on the semiconductor substrate at two sides of the first gate trench, and a first gate dielectric layer is separated between the word line gates and the semiconductor substrate; A sixth dielectric layer is isolated between the side surface of the first gate trench and the second side surface of the word line gate; An erase gate is formed in the top region of the floating gate and a second tunnel dielectric layer is spaced between the erase gate and the floating gate; A drain region is formed in a self-aligned manner in a surface region of the semiconductor substrate at a first side of the word line gate.
3. The super flash memory as claimed in claim 1, characterized in that: The first tunnel dielectric layer is a HTO oxide layer.
4. The super flash memory as claimed in claim 3, characterized in that: The third silicon nitride layer is an ALD silicon nitride layer; and the fifth silicon nitride layer is an ALD silicon nitride layer.
5. The super flash memory as claimed in claim 4, characterized in that: The thickness of the first tunnel dielectric layer is The thickness of the second oxide layer is The thickness of the third silicon nitride layer is The thickness of the fourth oxide layer is The thickness of the fifth silicon nitride layer is 6. The super flash memory as claimed in claim 1, characterized in that: The thickness of the TiN layer of the floating gate is 7. A method for manufacturing a super flash memory, characterized in that: The device unit is located in the storage area, and the steps of forming the device unit include: Step 1: forming a first gate trench, wherein the first gate trench is located at the top of the source region formation area, the bottom surface of the first gate trench is lower than the top surface of the semiconductor substrate, and the top surface of the first gate trench is higher than the top surface of the semiconductor substrate; Step 2: forming the source region in the surface area of the semiconductor substrate at the bottom of the first gate trench; Step 3: forming a first sidewall structure by self-alignment on the side of the first gate trench, including the following steps: Step 31, forming a first tunnel dielectric layer on the side and bottom surfaces of the first gate trench, forming a floating gate on the surface of the first tunnel dielectric layer, forming a second oxide layer on the surface of the floating gate, and forming a first stacked layer by stacking the first tunnel dielectric layer, the floating gate and the second oxide layer; the first stacked layer also extends to the surface outside the first gate trench; The material of the floating gate includes a TiN layer; The second oxide layer is an ALD oxide layer; Step 32, etching the second oxide layer, the floating gate and the first tunnel dielectric layer in sequence to form a first sidewall structure in self-alignment on the side of the first gate trench; The second side surface of the first spacer structure is formed by superposition of the second side surface of the second oxide layer and the etched surface of the floating gate and the first tunnel dielectric layer located at the bottom of the second side surface of the second oxide layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the first spacer structure; Step 4: forming a second sidewall structure by self-alignment on the second side of the first sidewall structure, including the following steps: Step 41, forming a third silicon nitride layer on the second side surface of the first spacer structure and the bottom surface of the first gate trench, forming a fourth oxide layer on the surface of the third silicon nitride layer, and forming a fifth silicon nitride layer on the surface of the fourth oxide layer; forming a second stacked layer by stacking the third silicon nitride layer, the fourth oxide layer and the fifth silicon nitride layer; the second stacked layer also extends to the top surface of the first spacer structure and the surface outside the first gate trench; The fourth oxide layer is a HTO oxide layer; The third silicon nitride layer serves as a protective layer of the floating gate to prevent the TiN layer of the floating gate from being oxidized; Step 42, etching the fifth silicon nitride layer, the fourth oxide layer and the third silicon nitride layer in sequence to form the second sidewall spacer structure by self-alignment; The second side surface of the second sidewall structure is formed by superimposing the second side surface of the fifth silicon nitride layer and the etched surfaces of the fourth oxide layer and the third silicon nitride layer located at the bottom of the second side surface of the fifth silicon nitride layer; the bottom surface of the first gate trench is exposed between the second side surfaces of the second sidewall structure.
8. The method for manufacturing a super flash memory as claimed in claim 7, wherein: In step 1, two word line gates are symmetrically arranged on the semiconductor substrate at two sides of the first gate trench, and a first gate dielectric layer is separated between the word line gates and the semiconductor substrate; A sixth dielectric layer is isolated between the side surface of the first gate trench and the second side surface of the word line gate; After step 4 is completed, the method further includes: step 5, filling a control gate in the first gate trench between the second side surfaces of the second spacer structure, wherein the control gate contacts the source region at the bottom; After step 5 is completed, it also includes: forming an erase gate and a second tunnel dielectric layer between the erase gate and the floating gate in a top region of the floating gate; After the first side of the word line gate is formed, the method further includes: A drain region is formed in a self-aligned manner in a surface region of the semiconductor substrate at a first side of the word line gate.
9. The method for manufacturing a super flash memory as claimed in claim 7, wherein: The first tunnel dielectric layer is a HTO oxide layer grown by a HTO process.
10. The method for manufacturing a super flash memory according to claim 9, wherein: The third silicon nitride layer is an ALD silicon nitride layer formed by an ALD process; and the fifth silicon nitride layer is an ALD silicon nitride layer formed by an ALD process.
11. The method for manufacturing a super flash memory according to claim 10, wherein: The thickness of the first tunnel dielectric layer is The thickness of the second oxide layer is The thickness of the third silicon nitride layer is The thickness of the fourth oxide layer is The thickness of the fifth silicon nitride layer is 12. The method for manufacturing a super flash memory as claimed in claim 9, wherein: The temperature of the HTO process of the first tunnel dielectric layer is 600° C. to 900° C.
13. The method for manufacturing a super flash memory according to claim 7, wherein: The TiN layer of the floating gate is formed by deposition using a PVD process.
14. The method for manufacturing a super flash memory according to claim 13, wherein: The temperature of the PVD process of the TiN layer of the floating gate is 400 degrees Celsius.
15. The method for manufacturing a super flash memory according to claim 13, wherein: The thickness of the TiN layer of the floating gate is 16. The method for manufacturing a super flash memory according to claim 7, wherein: A non-storage area is also included outside the storage area; In step 1, while forming the first gate trench, the method further includes forming a second gate trench in the non-storage area, wherein the second gate trench is located above a field oxide formed on the semiconductor substrate; In step 31, the first stacking layer is also formed on the inner surface of the second gate trench and the surface outside the second gate trench; In step 32, before performing the etching process of the first sidewall structure, the process further includes: forming a first mask layer covering the storage area and opening the non-storage area; Using the first mask layer as a mask, the first stacking layer in the non-storage area is removed; The first mask layer is removed by etching.
17. The method for manufacturing a super flash memory according to claim 7 or 16, characterized in that: In step 32, the process of etching the TiN layer of the floating gate in the first stacking layer adopts wet etching, and the wet etching solution adopts a mixed cleaning solution of HF, H2O2 and H2O.
18. The method for manufacturing a super flash memory according to claim 7, wherein: In step 42, an anisotropic dry etching process is used to etch the fifth silicon nitride layer, the fourth oxide layer and the third silicon nitride layer.