Modifier for polyacetal resin, polyacetal resin composition, and method for producing modifier for polyacetal resin

By using a modifier containing rubber graft copolymer and glycidyl polymer compound in the polyacetal resin, the concentration and pH of the modifier are controlled, and the VOC generation amount in the polyacetal resin composition is solved. Problem, a polyacetal resin composition with low VOC and high impact resistance and weather resistance is realized.

CN118946632APending Publication Date: 2024-11-12KANEKA CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030489.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyacetal resin compositions produce a high amount of volatile organic compounds (VOCs) during the molding process, which is difficult to meet the demand for low VOCs of automotive components, while taking into account both impact resistance and weather resistance.

Method used

Modifier for polyacetal resin containing a rubber graft copolymer containing a specific composition and a polymer compound having a glycidyl group is used to form a modifier through an emulsified state addition and coagulation process to control the chlorine and chlorine in the modifier. The calcium concentration and pH value form a polyacetal resin composition with excellent weather resistance and low VOC generation.

Benefits of technology

It realizes the reduction of VOC generation in automotive parts, while improving the impact resistance and weather resistance of polyacetal resin, providing a high level of molded body performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005060146180000361
    Figure BDA0005060146180000361
  • Figure BDA0005060146180000391
    Figure BDA0005060146180000391
  • Figure BDA0005060146180000401
    Figure BDA0005060146180000401
Patent Text Reader

Abstract

The present invention addresses the problem of providing a novel impact-resistant modifier for polyacetal resins, said impact-resistant modifier being capable of providing a polyacetal resin composition having a small amount of VOC generation. A modifier for polyacetal resins, which contains a rubber-containing graft copolymer (A) having a specific composition and a polymer compound (B) having a glycidyl group, the content of elemental chlorine and the content of elemental calcium in the modifier being within a specific range, and the pH of a mixture of the modifier and pure water being within a specific range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a modifier for polyacetal resin, a polyacetal resin composition and a method for producing the modifier for polyacetal resin. Background Art

[0002] Polyacetal resin is a crystalline engineering plastic. Due to its high crystallinity, it has excellent strength, sliding properties and dimensional stability. Therefore, polyacetal resin is widely used not only in housings, but also in electrical and electronic components such as resin gears, door handles, and clamps, and automotive parts. These resin parts are required to have high impact resistance, low wear resistance, low noise, etc., among which high impact resistance is emphasized.

[0003] In recent years, there has been a demand for automobile parts to be resin parts that generate less VOC (volatile organic compounds), and therefore, a resin composition that generates less VOC has been sought.

[0004] Currently, various modifiers for polyacetal and resin compositions containing the modifiers are being developed.

[0005] For example, Patent Document 1 discloses a composition containing polyoxymethylene, epoxidized fatty acid, a polymer stabilizer, and an impact resistance improver.

[0006] Patent Document 2 discloses a rubber graft polymer containing a rubber portion containing a diene structural unit. In the rubber graft polymer disclosed in Patent Document 2, the mass ratio of the rubber portion to the graft portion is 70 to 90 mass % of the rubber portion and 10 to 30 mass % of the graft portion. In addition, in the rubber graft polymer disclosed in Patent Document 2, the total amount of sulfate ions and sulfite ions contained in water extracted with hot water by a specific method is 3.5 ppm or less, the content of chloride ions is 150 ppm or less, and the total content of sodium ions and potassium ions is 20 ppm or less relative to the total amount of the rubber graft polymer.

[0007] Patent document 3 discloses a polyoxymethylene resin composition, characterized in that it contains (A) 100 parts by mass of a polyoxymethylene resin and (B) 0.5 to 50 parts by mass of a modifying material, wherein the (B) modifying material comprises (b-1) a thermoplastic polyurethane and (b-2) a grafted rubber copolymer, and the (b-2) grafted rubber copolymer has a structure of more than two layers.

[0008] Patent Document 4 discloses a resin composition comprising a polyacetal resin (A), a salt (B) composed of a carboxylic acid and an alkaline earth metal, and a rubber-containing graft copolymer (C).

[0009] Patent Document 5 discloses a polyacetal resin composition containing specific amounts of (A) a polyacetal polymer, (B) a hindered phenol-based antioxidant, (C) an aliphatic carboxylic acid hydrazide, (D) a hydantoin compound having two hydrazinocarbonylalkyl groups, (E) an alkaline earth metal salt of an aliphatic carboxylic acid, (F) a hindered amine compound, (G) an ultraviolet absorber, and (H) a core-shell polymer having a core of a rubber-like polymer and a shell of a glassy polymer composed of a vinyl copolymer.

[0010] For example, there is a technique such as Patent Document 6, but an improvement in the balance among impact strength, VOC, and weather resistance is required.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application No. 2008-504397

[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 2016-000828

[0015] Patent Document 3: Japanese Patent Application Laid-Open No. 2019-026810

[0016] Patent Document 4: International Publication No. WO2016 / 136726

[0017] Patent Document 5: Japanese Patent Application Laid-Open No. 2021-036018

[0018] Patent Document 6: Japanese Patent Application Laid-Open No. 2014-177647 Summary of the invention

[0019] However, from the viewpoint of the amount of VOC generated, the above-mentioned conventional techniques are not sufficient and there is room for further improvement.

[0020] One embodiment of the present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a novel modifier for polyacetal resin that can provide a polyacetal resin composition having excellent weather resistance and a low VOC generation amount.

[0021] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention by finding a new insight that an impact modifier for polyacetal resin that satisfies the following (A1) to (A3) has a low VOC generation amount: (A1) comprising a rubber-containing graft copolymer having a specific structure and a polymer compound having a glycidyl group, (A2) having a chlorine element concentration and a calcium element concentration within a specific range, and (A3) having a pH within a specific range.

[0022] That is, a modifier for polyacetal resin according to one embodiment of the present invention is a modifier for polyacetal resin, comprising a rubber-containing graft copolymer (A) and a polymer compound (B) having a glycidyl group, wherein the rubber-containing graft copolymer (A) has an elastomer and a graft portion graft-bonded to the elastomer, the graft portion is composed only of constituent units derived from a vinyl monomer having no reactive functional group, the mass ratio of the elastomer to the graft portion (part by mass of the elastomer / part by mass of the graft portion) is 60 / 40 to 95 / 5, the content of chlorine in the modifier for polyacetal resin is 1 ppm to 170 ppm based on the mass of the modifier for polyacetal resin, the content of calcium in the modifier for polyacetal resin is 1 ppm to 780 ppm based on the mass of the modifier for polyacetal resin, and the pH of a mixture consisting of 10 parts by mass of the modifier for polyacetal resin and 100 parts by mass of deionized water is 6.0 to 8.0.

[0023] In addition, a method for producing a modifier for polyacetal resin according to one embodiment of the present invention comprises: a polymer compound (B) adding step, in which a polymer compound (B) having a glycidyl group is added in an emulsified state to an aqueous latex containing a rubber-containing graft copolymer (A); a coagulation step, in which calcium chloride is added to the aqueous latex obtained in the polymer compound (B) adding step to obtain a coagulation body containing the rubber-containing graft copolymer (A) and the polymer compound (B); and a washing step, in which the coagulation body obtained in the coagulation step is washed; the rubber-containing graft copolymer (A) has an elastomer and a graft portion graft-bonded to the elastomer, the graft portion being composed only of constituent units derived from a vinyl monomer having no reactive functional group, the mass ratio of the elastomer to the graft portion (mass part of the elastomer / mass part of the graft portion) is 60 / 40 to 95 / 5, and the pH of the aqueous latex is 5 to 9.

[0024] According to one embodiment of the present invention, there is provided an effect of being able to provide a novel modifier for polyacetal resin that can provide a polyacetal resin composition having excellent weather resistance and a low VOC generation amount. DETAILED DESCRIPTION

[0025] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto. The present invention is not limited to the various configurations described below, and various changes can be made within the scope indicated in the scope of the request. In addition, embodiments or embodiments obtained by appropriately combining the technical means respectively disclosed in different embodiments or embodiments are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means respectively disclosed in each embodiment. It should be noted that all academic documents and patent documents recorded in this specification are cited as references in this specification. In addition, as long as there is no special explanation in this specification, "A to B" indicating a numerical range means "Above A (including A and greater than A) and below B (including B and greater than B)".

[0026] In this specification, a repeating unit derived from N monomers may be referred to as “N unit.” A repeating unit may also be referred to as a constitutional unit.

[0027] In addition, unless otherwise specified in this specification, M 1 Unit, M 2 Unit, ... and M n A copolymer having a unit (n is an integer greater than 2) as a constituent unit is referred to as M 1 / M 2 / … / M n Copolymer. As M 1 / M 2 / … / M n The copolymer, except for the cases explicitly stated, has no particular limitation on the polymerization method and may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer. 1 Unit, M 2 Unit, ... and M n The elastomer having a unit (n is an integer greater than 2) as a constituent unit is referred to as M 1 / M 2 / … / M n rubber.

[0028] [1. Technical concept of one embodiment of the present invention]

[0029] One of the above VOCs is formaldehyde. VDA275, one of the German automotive standards, describes a method for measuring formaldehyde released from resin parts (molded products). In recent years, the amount of VOC generated in the measurement methods unified based on these standards has been discussed.

[0030] Polyacetal resin is sensitive to the pH and / or residual ion amount of additives. Depending on the pH and / or residual ion amount, polyacetal may decompose during the processing of polyacetal resin to produce formaldehyde that is toxic to the human body. Since these additives and / or residual ions also remain in the molded body of polyacetal resin, the formaldehyde released from the molded body of polyacetal resin in a confined space becomes a problem. On the other hand, polyacetal sometimes requires various physical properties (such as impact resistance, etc.). Therefore, as a modifier for polyacetal resin, a modifier corresponding to various purposes such as improvement of impact resistance may be required. When a modifier manufactured using anionic emulsifiers and coagulants is added to polyacetal resin, the amount of formaldehyde generated from the polyacetal resin composition or its molded body is large, and this amount is particularly not allowed as the amount of formaldehyde for automotive use. For example, in the modifiers of the above-mentioned patent documents 1 to 6, when the modifier is combined with the polyacetal resin, the amount of VOC generated when the polyacetal resin composition is molded cannot be fully prevented or reduced.

[0031] Therefore, the present inventors have conducted intensive research for the purpose of providing a polyacetal resin modifier capable of providing a polyacetal resin composition with low VOC generation. As a result, as described above, the present inventors have found a new insight that the impact modifier for polyacetal resin that satisfies the above (A1) to (A3) generates low VOC even when it is mixed with a polyacetal resin, thereby completing the present invention.

[0032] In addition to the above-mentioned purpose, one embodiment of the present invention further takes the following (a), (b) and / or (c) as additional purposes that are preferably achieved: (a) providing a polyacetal resin modifier useful for achieving both high impact resistance of polyacetal resin and low formaldehyde generation at a higher level; (b) providing a polyacetal resin modifier that can prevent or reduce formaldehyde generated during and after molding of a polyacetal resin composition (including the resulting molded body) and further impart impact resistance, and a polyacetal resin composition containing the polyacetal resin modifier; and (c) providing a polyacetal resin modifier that can provide a molded body with excellent softness, and a polyacetal resin composition containing the polyacetal resin modifier.

[0033] The present inventors have conducted intensive studies to achieve the above additional object and have found that the use of a specific polyacetal resin modifier can achieve both high impact resistance of the polyacetal resin composition and prevention or reduction of the VOC amount during and after molding at a higher level.

[0034] According to one embodiment of the present invention, there can be provided (a) a polyacetal resin modifier comprising a rubber-containing graft copolymer useful for achieving both the impact resistance of a polyacetal resin and the prevention or reduction of formaldehyde generation at a higher level; (b) a polyacetal resin modifier capable of preventing or reducing the amount of formaldehyde generated during and after molding of a polyacetal resin composition and further capable of imparting impact resistance, and a polyacetal resin composition comprising the polyacetal resin modifier; and / or (c) a polyacetal resin modifier capable of providing a molded body having excellent softness, and a polyacetal resin composition comprising the polyacetal resin modifier.

[0035] 〔2. Modifier for polyacetal resin〕

[0036] A modifier for polyacetal resin according to one embodiment of the present invention comprises a rubber-containing graft copolymer (A) and a polymer compound (B) having a glycidyl group, wherein the rubber-containing graft copolymer (A) comprises an elastomer and a graft portion graft-bonded to the elastomer, the graft portion being composed only of constituent units derived from a vinyl monomer having no reactive functional group, the mass ratio of the elastomer to the graft portion (part by mass of the elastomer / part by mass of the graft portion) being 60 / 40 to 95 / 5, the content of chlorine in the modifier for polyacetal resin being 1 ppm to 170 ppm based on the mass of the modifier for polyacetal resin, the content of calcium in the modifier for polyacetal resin being 1 ppm to 780 ppm based on the mass of the modifier for polyacetal resin, and the pH of a mixture consisting of 10 parts by mass of the modifier for polyacetal resin and 100 parts by mass of deionized water being 6.0 to 8.0.

[0037] Hereinafter, the "modifier for polyacetal resin" may be referred to as "modifier". Hereinafter, the "modifier for polyacetal resin according to one embodiment of the present invention" may be referred to as "this modifier". When this modifier is mixed with the polyacetal resin (C) described later, a polyacetal resin composition is obtained. Hereinafter, the "polyacetal resin composition" may be referred to as "resin composition".

[0038] Since the present modifier has the above-mentioned structure, it has the advantage of being able to provide a polyacetal resin composition with a small amount of VOC generation. Specifically, the present modifier can provide a polyacetal resin composition with a small amount of VOC generation during and after the molding of the polyacetal resin composition. In addition, the present modifier also has the advantage of being able to provide a polyacetal resin composition that can provide excellent weather resistance and a polyacetal resin composition that can provide a molded body with excellent weather resistance. In addition, the present modifier also has the advantage of being able to provide a polyacetal resin composition that can provide a molded body with excellent impact resistance. In addition, the present modifier also has the advantage of being able to take into account (a) the high impact resistance of the molded body of the polyacetal resin composition and (b) preventing or reducing the amount of VOC generation during and after the molding of the polyacetal resin composition at a high level. In addition, the present modifier also has the advantage of being able to provide a polyacetal resin composition that can provide a molded body with excellent softness. It should be noted that in the technical field of polyacetal resins or polyacetal resin compositions, the amount of formaldehyde generated may become the most important problem as the amount of VOC generated. Therefore, in one embodiment of the present invention, the VOC is formaldehyde.

[0039] In this specification, the weatherability of the resin composition and the molded body is evaluated by the crack generation time during the weatherability test of the resin composition and the molded body. In this specification, the impact resistance of the molded body is evaluated by the notched Charpy impact value of the molded body. In this specification, the softness of the molded body is evaluated by the bending elastic modulus of the molded body. The method for measuring the crack generation time during the weatherability test of the resin composition and the molded body, and the method for measuring the notched Charpy impact value and the bending elastic modulus of the molded body are described in detail in the following examples.

[0040] (2-1. Rubber-containing graft copolymer (A))

[0041] The rubber-containing graft copolymer (A) contained in the present modifier has an elastomer and a graft portion graft-bonded to the elastomer.

[0042] (Elastomer)

[0043] As the elastomer, there can be mentioned an elastomer containing one or more selected from natural rubber, diene rubber, (meth)acrylate rubber and polyorganosiloxane rubber. The elastomer preferably contains one or more selected from diene rubber, (meth)acrylate rubber and polyorganosiloxane rubber, more preferably contains (meth)acrylate rubber, and further preferably consists only of (meth)acrylate rubber. According to this constitution, there is an advantage that the weather resistance of the polyacetal resin composition can be maintained in an excellent state.

[0044] ((Meth)acrylate rubber)

[0045] The (meth)acrylate rubber is an elastomer containing, as a constituent unit, a constituent unit derived from a (meth)acrylate monomer (a (meth)acrylate unit).

[0046] In this specification, "(meth)acrylate" means "methacrylate" and / or "acrylate", and "(meth)acrylic acid" means "methacrylic acid" and / or "acrylic acid". For example, "methyl (meth)acrylate" means "methyl methacrylate" and / or "methyl acrylate".

[0047] Examples of the (meth)acrylate monomers include (a) alkyl (meth)acrylates having an alkyl group having 1 to 22 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (b) (meth)acrylates containing an aromatic ring, such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; (c) hydroxyalkyl (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate; (d) glycidyl (meth)acrylates, such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; and (e) alkoxyalkyl (meth)acrylates. These (meth)acrylate monomers may be used alone or in combination of two or more.

[0048] The (meth)acrylate rubber may further contain, as a constituent unit, a constituent unit derived from a vinyl monomer other than the (meth)acrylate monomer copolymerizable with the (meth)acrylate monomer. Examples of the vinyl monomer other than the (meth)acrylate monomer copolymerizable with the (meth)acrylate monomer include (a) diene monomers and (b) monomers other than the (meth)acrylate monomer among the vinyl monomers.

[0049] The (meth)acrylate rubber preferably further comprises constituent units derived from a cross-linking agent and / or a graft cross agent. In other words, in the manufacturing process of the (meth)acrylate rubber, a cross-linking agent and / or a graft cross agent is preferably used. When the (meth)acrylate rubber further comprises constituent units derived from a cross-linking agent and / or a graft cross agent, the grafting rate described later becomes higher. As a result, there is the following advantage: in the polyacetal resin composition obtained by kneading the modifier with the polyacetal resin, the dispersibility of the rubber-containing graft copolymer (A) in the polyacetal resin is good.

[0050] Examples of crosslinking agents and grafting agents include (a) allyl (meth)acrylates such as allyl (meth)acrylate and allyl (meth)acrylates; (b) polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; and (c) polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. These crosslinking agents and grafting agents may be used alone or in combination of two or more.

[0051] Preferred examples of the (meth)acrylate rubber include acrylate rubbers such as polybutyl acrylate rubber and butyl acrylate / 2-ethylhexyl acrylate copolymer. Polybutyl acrylate rubber is an elastomer containing 50 to 100% by mass of butyl acrylate units in 100% by mass of the constituent units.

[0052] Examples of the diene rubber and the polyorganosiloxane rubber include conventionally known rubbers (for example, butadiene rubber and silicone rubber, respectively).

[0053] In one embodiment of the present invention, the elastomer preferably contains 50% by mass or more of butyl acrylate units in 100% by mass of the elastomer, more preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, further preferably 90% by mass or more, and particularly preferably 95% by mass or more. This configuration has the advantage of a good balance among economy, weather resistance, and low elastic modulus.

[0054] The "elastomer" of the rubber-containing graft copolymer (A) may consist of only one type of elastomer (polymer) having the same composition of constituent units, or may consist of a plurality of types of elastomers (polymers) having different compositions of constituent units.

[0055] (Grafting)

[0056] The grafted portion is composed only of constituent units derived from vinyl monomers having no reactive functional groups (e.g., hydroxyl, carboxyl, epoxy, amide, oxirane, etc.). In this specification, "constituent units derived from vinyl monomers having no reactive functional groups" are sometimes referred to as "constituent units U". The grafted portion is composed only of constituent units U, which has the following advantages: (a) the reaction between the reactive functional groups of the rubber-containing graft copolymer (A) and (b) the reaction between the reactive functional groups in the polyacetal resin composition and the polyacetal resin can be eliminated, and the gloss (gloss) of the surface of the molded body will not be reduced.

[0057] Examples of the vinyl monomer having no reactive functional group that is a source of the structural unit U include aromatic vinyl compounds having no reactive functional group (for example, styrene monomers such as styrene), vinyl cyanide compounds (for example, acrylonitrile and methacrylonitrile), and unsaturated carboxylic acid esters.

[0058] As the unsaturated carboxylic acid ester having no reactive functional group, there can be mentioned acrylate and methacrylate etc. which have alkyl esters having 1 to 12 carbon atoms. As the unsaturated carboxylic acid ester having no reactive functional group, there can be mentioned methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate and butyl methacrylate etc. more specifically.

[0059] As the vinyl monomer having no reactive functional group, further suitable examples include ester (meth)acrylates having an alkyl group having 1 to 22 carbon atoms and an alkoxy group, such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate.

[0060] In the polymerization of the graft portion, when selecting the monomers to be used, it is preferred to consider the type of the polyacetal resin (C) to be mixed with the modifier containing the obtained rubber-containing graft copolymer (A) (i.e., to be modified). For example, in the selection of the monomers in the polymerization of the graft portion, it is preferred to consider (a) the compatibility of the polyacetal resin (C) and the obtained rubber-containing graft copolymer (A), (b) the refractive index of the polyacetal resin composition obtained by mixing the modifier containing the rubber-containing graft copolymer (A) with the polyacetal resin (C), and the like, and select any one monomer or use any two or more monomers in combination at any mixing ratio.

[0061] The graft portion is preferably composed of constituent units U derived from at least one monomer selected from (meth)acrylate monomers and styrene monomers, more preferably composed of constituent units derived from at least one monomer selected from methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate and styrene monomers, more preferably composed of constituent units derived from at least one monomer selected from methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate and styrene, further preferably composed of constituent units derived from at least one monomer selected from methyl acrylate, methyl methacrylate, ethyl acrylate and butyl acrylate, particularly preferably composed of constituent units derived from at least one of methyl methacrylate and butyl acrylate, and most preferably composed of constituent units derived from methyl methacrylate and butyl acrylate. According to this constitution, there are advantages that a rubber-containing graft copolymer (A) having good granulation properties and less odor during production can be obtained, and the molded article of the obtained polyacetal resin composition has excellent weather resistance.

[0062] The graft portion preferably contains 50% by mass or more of constituent units derived from methyl methacrylate and constituent units derived from butyl acrylate in total, more preferably 70% by mass or more, further preferably 85% by mass or more, and particularly preferably 95% by mass or more, in 100% by mass of the graft portion. This constitution has the advantage that the granulation property during the production of the rubber-containing graft copolymer (A) is good.

[0063] The "graft portion" of the rubber-containing graft copolymer (A) may consist of only one type of graft portion (polymer) having the same constituent unit composition, or may consist of a plurality of types of graft portions (polymers) having different constituent unit compositions.

[0064] The mass ratio of the elastomer to the graft part in the rubber-containing graft copolymer (A) (mass part of the elastomer / mass part of the graft part) is 60 / 40 to 95 / 5, preferably 65 / 35 to 90 / 10, more preferably 70 / 30 to 85 / 15, further preferably 70 / 35 to 80 / 20, and particularly preferably 70 / 35 to 75 / 25. This configuration has the following advantages: the rubber-containing graft copolymer (A) in the modifier has excellent compatibility with the polyacetal resin (C), and the molded body of the polyacetal resin composition has excellent impact resistance.

[0065] (Method for producing rubber-containing graft copolymer (A))

[0066] As a method for producing the rubber-containing graft copolymer (A), any of bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization may be adopted, but emulsion polymerization, i.e., emulsion graft polymerization, is preferred. Specifically, as an example, (1) water and an emulsifier are added to a reaction vessel equipped with a stirrer, and a monomer mixture for forming an elastomer and a polymerization initiator are further added, and a chain transfer agent and / or a redox agent are added as required, and the obtained raw material solution is heated and stirred to polymerize to form an elastomer, and then (2) a monomer mixture for forming a graft portion is added to the reaction solution (suspension) containing the elastomer, and an emulsifier, a polymerization initiator, a chain transfer agent, and / or a redox agent are further added to the reaction solution as required, and the reaction solution is heated and stirred to polymerize to form a graft portion.

[0067] The types of emulsifiers, polymerization initiators, chain transfer agents and redox agents used herein are not particularly limited, and known substances can be used. In addition, the method of adding each raw material to the reaction vessel is also not particularly limited, and in addition to adding it all at once before the start of polymerization, it can also be added in batches. In addition, the polymerization of the graft portion can be carried out in one or more stages, and the monomer components of each stage can be the same or different. In the polymerization of the graft portion, the monomers forming the graft portion can be added all at once in a short period of time, or they can be added continuously in a certain amount each time over a certain period of time, or they can be combined.

[0068] When the emulsion polymerization method is used as the method for producing the rubber-containing graft copolymer (A), a known polymerization initiator can be used, for example, a known thermal decomposition type polymerization initiator such as 2,2'-azobisisobutyronitrile, hydrogen peroxide, potassium persulfate, ammonium persulfate, etc.

[0069] In the production of the rubber-containing graft copolymer (A), a redox initiator can also be used. The redox initiator is an initiator that uses (a) a peroxide such as an organic peroxide and an inorganic peroxide and (b) a reducing agent such as sodium formaldehyde sulfoxylate and glucose as required, and a transition metal salt such as iron (II) sulfate as required, a chelating agent such as disodium ethylenediaminetetraacetic acid as required, and a phosphorus-containing compound such as sodium pyrophosphate as required. Examples of organic peroxides include tert-butyl peroxyisopropyl carbonate, p-menthane hydroperoxide, isopropylbenzene hydroperoxide, diisopropylbenzene peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-hexyl peroxide, and the like. Examples of inorganic peroxides include hydrogen peroxide, potassium persulfate, and ammonium persulfate.

[0070] In the production of the rubber-containing graft copolymer (A), a surfactant may be used in addition to the above components. The type and amount of the surfactant used are within known ranges.

[0071] In the production of the rubber-containing graft copolymer (A), conditions such as polymerization temperature, pressure, and deoxidation during polymerization can be those within known ranges.

[0072] (2-2. Polymer compound having a glycidyl group (B))

[0073] The modifier includes a polymer compound (B) having a glycidyl group. The polymer compound (B) having a glycidyl group can play a great role in providing the modifier with a polyacetal resin composition with a low VOC generation amount. In this specification, the "polymer compound (B) having a glycidyl group" is sometimes referred to as "polymer compound (B)".

[0074] (a) During the molding of the polyacetal resin composition, for example, when the polyacetal resin composition is extruded and further molded, and / or (b) after the molding of the polyacetal resin composition, the formaldehyde that may be generated may be further oxidized to become formic acid. Formic acid further promotes the decomposition of the polyacetal resin composition, that is, the generation of formaldehyde. The polymer compound (B) contained in the modifier can react with the formic acid in the polyacetal resin composition when the modifier is added to the polyacetal resin composition to render the formic acid non-toxic. Therefore, the polymer compound (B) can also be called a formic acid scavenger.

[0075] Examples of the polymer compound (B) include (a) epoxidized fats and oils such as epoxidized soybean oil, epoxidized castor oil, and epoxidized linseed oil, (b) epoxidized fatty acid esters, (c) epoxy resins, and (d) liquid polymers having a glycidyl group. Examples of the epoxidized fatty acid esters include epoxidized fatty acid butyl ester, epoxidized fatty acid 2-ethylhexyl ester, epoxidized fatty acid octyl ester, and epoxidized fatty acid alkyl ester.

[0076] Epoxidized fats and oils and epoxidized fatty acid esters are sometimes referred to as epoxy plasticizers. That is, in this specification, epoxy plasticizers are also included in the polymer compound (B). Examples of epoxy plasticizers other than epoxidized fats and oils and epoxidized fatty acid esters include diepoxystearyl hexahydrophthalate and di-2-ethylhexyl hexahydrophthalate.

[0077] The polymer compound (B) is preferably an epoxidized oil or fat, more preferably at least one selected from epoxidized soybean oil, epoxidized castor oil, and epoxidized linseed oil, further preferably at least one of epoxidized soybean oil and epoxidized castor oil, and particularly preferably epoxidized soybean oil. This configuration has the advantages of excellent economic efficiency and the advantages of being able to easily obtain an aggregate of the polymer compound (B) having a high affinity for the rubber-containing graft copolymer (A) and existing near the rubber-containing graft copolymer (A) (for example, an aggregate of the polymer compound (B) existing between a plurality of particles of the rubber-containing graft copolymer (A)).

[0078] The content of the polymer compound (B) in the present modifier is not particularly limited. In the present modifier, the content of the polymer compound (B) is preferably 0.1 to 5.0 parts by mass, more preferably 0.1 to 4.5 parts by mass, more preferably 0.5 to 4.0 parts by mass, more preferably 0.5 to 3.5 parts by mass, and particularly preferably 1.0 to 3.0 parts by mass, relative to 100 parts by mass of the rubber-containing graft copolymer (A). According to this structure, the obtained modifier has the advantage that it can provide a polyacetal resin composition with less VOC generation.

[0079] (2-3. Other optional ingredients)

[0080] The present modifier may contain other optional components other than the above components within a range that does not impair the effects of one embodiment of the present invention. Examples of other optional components include anti-blocking agents, antioxidants described below, and various components described in the section (4-4. Other additives) described below.

[0081] Other optional components can be appropriately added in any process of the manufacturing method of the present modifier. For example, other optional components can be added to the water suspension (aqueous latex) before or after the coagulation of the rubber-containing graft copolymer (A). In addition, other optional components can be added to the modifier.

[0082] (2-4. Chlorine content)

[0083] When the modifier is mixed with a polyacetal resin to form a polyacetal resin composition, the chlorine element present in the modifier can induce the decomposition of the polyacetal resin in the polyacetal resin composition. Therefore, the less chlorine element present in the modifier, the better. Based on the mass of the modifier, the content of chlorine element in the modifier is 1ppm to 170ppm, preferably 1ppm to 160ppm, further preferably 1ppm to 150ppm, and particularly preferably 1ppm to 140ppm. According to this composition, the obtained modifier can provide a polyacetal resin composition with less VOC generation. It should be noted that, as described later, when a coagulant containing chlorine element is used in the method for manufacturing the modifier, the obtained modifier may contain chlorine element. The content of chlorine in the modifier can be adjusted by changing (a) the amount of the coagulant containing chlorine used in the method for producing the modifier, and / or (b) the washing conditions (such as the temperature of the washing water, the number of washing times and the amount of the washing water) of the agglomerate containing the rubber-containing graft copolymer (A) and the polymer compound (B) in the method for producing the modifier.

[0084] (2-5. Calcium content)

[0085] When the modifier is mixed with a polyacetal resin to form a polyacetal resin composition, the calcium element present in the modifier can induce the decomposition of the polyacetal resin in the polyacetal resin composition. Therefore, the less calcium element present in the modifier, the better. Based on the mass of the modifier, the content of calcium element in the modifier is 1ppm to 780ppm, preferably 1ppm to 770ppm, further preferably 1ppm to 760ppm, and particularly preferably 1ppm to 750ppm. According to this composition, the obtained modifier can provide a polyacetal resin composition with less VOC generation. It should be noted that, as described later, when a coagulant containing calcium element is used in the method for manufacturing the modifier, the obtained modifier may contain calcium element. The content of calcium element in the modifier can be adjusted by changing (a) the amount of the coagulant containing calcium element used in the method for producing the modifier, (b) the washing conditions (such as the temperature of the washing water, the number of washing times and the amount of the washing water) of the agglomerate containing the rubber-containing graft copolymer (A) and the polymer compound (B) in the method for producing the modifier, etc.

[0086] (2-6.pH)

[0087] The pH of a mixture consisting of 10 parts by mass of the present modifier and 100 parts by mass of deionized water is 6.0 to 8.0. In other words, the present modifier is neutral or weakly alkaline. According to this configuration, the obtained modifier has the advantage of being able to provide a polyacetal resin composition with a lower VOC generation amount.

[0088] (2-7. Epoxy content)

[0089] The epoxy group content in the present modifier is not particularly limited, but is preferably 15 μmol / g to 180 μmol / g, more preferably 20 μmol / g to 170 μmol / g, more preferably 25 μmol / g to 160 μmol / g, more preferably 30 μmol / g to 150 μmol / g, more preferably 30 μmol / g to 140 μmol / g, further preferably 30 μmol / g to 130 μmol / g, and particularly preferably 35 μmol / g to 125 μmol / g. According to this configuration, the obtained modifier has the advantage of being able to provide a polyacetal resin composition with a lower VOC generation amount.

[0090] It should be noted that the epoxy group content (mol / g) in the modifier refers to the ratio of the total amount (mol) of (i) the epoxy group content contained in the rubber-containing graft copolymer (for example, when a monomer containing an epoxy group is used in the production of the rubber-containing graft copolymer, the obtained rubber-containing graft copolymer contains epoxy groups), (ii) the epoxy group content contained in the polymer compound (B), and (iii) the epoxy group content contained in other components to the total mass (g) of the modifier.

[0091] [3. Method for producing a modifier for polyacetal resin]

[0092] The method for producing a modifier for polyacetal resin according to one embodiment of the present invention comprises: a polymer compound (B) adding step, in which a polymer compound (B) having a glycidyl group is added in an emulsified state to an aqueous latex containing a rubber-containing graft copolymer (A); a coagulation step, in which calcium chloride is added to the aqueous latex obtained in the polymer compound (B) adding step to obtain a coagulation body containing the rubber-containing graft copolymer (A) and the polymer compound (B); and a washing step, in which the coagulation body obtained in the coagulation step is washed; the rubber-containing graft copolymer (A) has an elastomer and a graft portion graft-bonded to the elastomer, the graft portion is composed only of constituent units derived from a vinyl monomer having no reactive functional group, the mass ratio of the elastomer to the graft portion (mass part of the elastomer / mass part of the graft portion) is 60 / 40 to 95 / 5, and the pH of the aqueous latex is 5 to 9.

[0093] Hereinafter, “the method for producing a polyacetal resin modifier according to one embodiment of the present invention” may be referred to as “the present production method”.

[0094] The present inventors have unexpectedly independently found, during intensive research, that a polyacetal resin modifier capable of providing a polyacetal resin composition with a low VOC generation amount can be provided by adopting a production method having the following structures (c1) and (c2):

[0095] (c1) before obtaining the agglomerate of the rubber-containing graft copolymer (A), adding the polymer compound (B) to the aqueous latex of the rubber-containing graft copolymer (A); and

[0096] (c2) The polymer compound (B) is added in an emulsified state to the aqueous latex containing the rubber graft copolymer (A).

[0097] The reason why a modifier for polyacetal resin according to one embodiment of the present invention can be provided by having the above-mentioned structures (c1) and (c2) is not yet clear, but it is presumed as follows: In the present production method (particularly the polymer compound (B) adding step), by implementing the above-mentioned (c1) and (c2), it is possible to obtain agglomerates of the polymer compound (B) in the vicinity of the rubber-containing graft copolymer (A) (for example, agglomerates in which the polymer compound (B) enters between particles of a plurality of rubber-containing graft copolymers (A)). Therefore, in the modifier finally obtained, the polymer compound (B) exists in the vicinity of the rubber-containing graft copolymer (A). Furthermore, in the polyacetal resin composition obtained by mixing the modifier with the polyacetal resin (for example, kneading), the polymer compound (B) also exists in the vicinity of the rubber-containing graft copolymer (A). As a result, the VOC generation amount of the polyacetal resin composition during and after the molding of the polyacetal resin composition is reduced.

[0098] It should be noted that the present invention is not limited by the above speculation at all.

[0099] In the past, there are known modifiers (hereinafter also referred to as conventional modifiers) that contain a rubber-containing polymer but do not contain a polymer compound (B) having a glycidyl group. By mixing the above-mentioned conventional modifier, a polyacetal resin and a polymer compound (B) having a glycidyl group, a polyacetal resin composition containing a rubber-containing polymer and a polymer compound (B) having a glycidyl group can be obtained. However, the present inventors have independently obtained the following insight: the polyacetal resin composition obtained by using the conventional modifier and by such a method cannot reduce the amount of VOC generated during and after the molding of the polyacetal resin composition. It is speculated that this is because when using the conventional modifier and obtaining the polyacetal resin composition by the above method, the polymer compound (B) cannot be uniformly dispersed in the polyacetal resin, and as a result, the polymer compound (B) cannot exist near the rubber-containing graft copolymer (A).

[0100] That is, since the present manufacturing method has the above-mentioned structure (especially structures (c1) and (c2)), it has the following advantages: it is possible to provide a modifier that can provide a polyacetal resin composition with a low VOC generation. Specifically, the modifier obtained by the present manufacturing method can provide a polyacetal resin composition with a low VOC generation during and after the molding of the polyacetal resin composition. In addition, the modifier obtained by the present manufacturing method also has the following advantages: it is possible to provide a polyacetal resin composition that can provide excellent weather resistance and a polyacetal resin composition that can provide a molded body with excellent weather resistance. In addition, the modifier obtained by the present manufacturing method also has the following advantages: it is possible to provide a polyacetal resin composition that can provide a molded body with excellent impact resistance. In addition, the modifier obtained by the present manufacturing method also has the following advantages: it is possible to take into account at a high level (a) the high impact resistance of the molded body of the polyacetal resin composition and (b) the prevention or reduction of the VOC generation during and after the molding of the polyacetal resin composition. In addition, the modifier obtained by the present production method has an advantage of being able to provide a polyacetal resin composition that can provide a molded product having excellent flexibility.

[0101] Hereinafter, each mode of the present production method will be described in detail, but matters other than those described below (such as each mode containing the rubber graft copolymer (A) and the polymer compound (B)) are not particularly limited, and the description of the above-mentioned item [2. Modifier for polyacetal resin] is appropriately cited.

[0102] (Process for preparing rubber-containing graft copolymer (A))

[0103] The present production method may also include a step of preparing a rubber-containing graft copolymer (A) for preparing an aqueous latex containing the rubber-containing graft copolymer (A) before the step of adding the polymer compound (B). As a specific embodiment of the step of preparing the rubber-containing graft copolymer (A), for example, there may be mentioned a method of producing the rubber-containing graft copolymer (A) by emulsion polymerization. As a specific example of a method of producing the rubber-containing graft copolymer (A) by emulsion polymerization, it is the same as the production method already described in the above-mentioned item (method of producing the rubber-containing graft copolymer (A)), so the description is cited and omitted here. When the rubber-containing graft copolymer (A) is produced by emulsion polymerization, the aqueous latex containing the rubber-containing graft copolymer (A) may contain an emulsifier.

[0104] (Polymer Compound (B) Adding Step)

[0105] The polymer compound (B) adding step can also be said to include a step of adding the rubber-containing graft copolymer (A) and the aqueous latex containing the polymer compound (B).

[0106] “Adding the polymer compound (B) in an emulsified state” can also be referred to as “adding an emulsion of the polymer compound (B)”. The method for obtaining the emulsion of the polymer compound (B) is not particularly limited, and examples thereof include (a) a method of forcibly emulsifying water, an emulsifier and a polymer compound (B) by stirring them; and (b) a method of mixing the polymer compound (B) with a reactive emulsifier to react the reactive group of the polymer compound (B) with the reactive emulsifier to obtain a polymer compound (B) having an emulsifying ability, and then dispersing the polymer compound (B) in water. From the viewpoint of industrial ease, as a method for obtaining an emulsion of the polymer compound (B), the method (a) obtained by stirring water, an emulsifier and a polymer compound (B) is preferred.

[0107] (Coagulation process)

[0108] The coagulation step is a step of obtaining a coagulation body composed of the rubber-containing graft copolymer (A) and the polymer compound (B) using calcium chloride.

[0109] In the coagulation process, the emulsifier and calcium chloride react in the aqueous latex to produce a salt as a reaction product. Therefore, calcium chloride can also be said to be a coagulant.

[0110] The present inventors have independently found that when a coagulant such as calcium chloride is used to obtain an aggregate, the obtained modifier can provide a polyacetal resin composition with a smaller amount of VOC generation than when the aggregate is obtained by freeze-drying without using a coagulant.

[0111] In addition, the present inventors independently obtained the following knowledge: when a coagulant other than calcium chloride (e.g., magnesium chloride) is used to obtain an aggregate without using calcium chloride, it is difficult to prevent or reduce the amount of VOC generated during and after molding of the polyacetal resin composition provided by the obtained modifier. The knowledge that the type of coagulant used when obtaining an aggregate containing a rubber graft copolymer affects the amount of VOC generated during and after molding of the finally obtained polyacetal resin composition is a knowledge that was completely unthinkable before and can be said to be a surprising knowledge.

[0112] The amount of the coagulant used in the aggregation step is not particularly limited, but is preferably 0.1 to 10.0 parts by mass, particularly preferably 1.0 to 8.0 parts by mass, based on 100 parts by mass of the total amount of the rubber-containing graft copolymer (A) and the polymer compound (B) in the aqueous latex.

[0113] (Cleaning process)

[0114] The washing step is a step of removing impurities from the aggregate. Examples of the impurities include salts that are reaction products of the emulsifier and the coagulant generated in the aggregation step.

[0115] The lower the conductivity of the washing water, the more preferred. The conductivity (mS / m) of the washing water is preferably 0.01mS / m to 1.00mS / m, more preferably 0.01mS / m to 0.80mS / m, further preferably 0.01mS / m to 0.50mS / m, and particularly preferably 0.01mS / m to 0.30mS / m. According to this configuration, there is an advantage that the obtained modifier can provide a polyacetal resin composition with a lower VOC generation amount.

[0116] Since the washing water has low conductivity, pure water (conductivity of 0.01 mS / m to 1.00 mS / m) and deionized water (conductivity of 0.01 mS / m to 0.30 mS / m) are preferable.

[0117] The amount of the washing water is not particularly limited, but is, for example, preferably 500 to 50,000 parts by mass, more preferably 500 to 10,000 parts by mass, and particularly preferably 500 to 5,000 parts by mass, based on 100 parts by mass of the aggregates.

[0118] The method for washing the agglomerates in the washing step is not particularly limited. As the method for washing the agglomerates, for example, a method of mixing the agglomerates and water and stirring them with a stirrer, a method of kneading the agglomerates and water with a kneader, a method of mixing the agglomerates and water with a rotation and revolution mixer, a method of spraying water onto the agglomerates, a method of washing the filter cake with a pressure filter, etc. can be cited. As the kneading machine, various kneading machines such as a batch kneading machine, a continuous kneading machine, an extrusion kneading machine, and an extruder can be used.

[0119] The number of times the agglomerates are washed in the washing step is not particularly limited, and the washing may be performed once or a plurality of times. The washing time for each washing step is also not particularly limited.

[0120] In the washing step, the method for removing the washing water is not limited, and examples thereof include drainage of the washing water, vacuum filtration, oil-water separation, filter press, centrifugal separation, belt press, screw press, membrane separation, and squeeze dehydration.

[0121] The method for dehydrating the aggregate is not particularly limited, and examples thereof include vacuum filtration, oil-water separation, filter press, centrifugal separation, belt press, screw press, membrane separation, and squeeze dehydration.

[0122] The present production method may further include a step of drying the aggregate containing the rubber-containing graft copolymer (A) and the polymer compound (B) obtained through the washing step.

[0123] There are no particular limitations on the specific method of the drying process, and examples include a method of drying the agglomerates using a dryer, a method of placing the agglomerates in a container and heating and reducing the pressure in the container, a method of placing the agglomerates in a container and bringing a dry gas into convection contact with the agglomerates in the container, etc. There are no particular limitations on the drying temperature in the drying process, such as the temperature in the dryer or the temperature of the drying gas.

[0124] The agglomerates of the rubber-containing graft copolymer (A) and the polymer compound (B) obtained by the present production method (or their dried products) can be used directly as a modifier for polyacetal resin. Alternatively, the agglomerates of the rubber-containing graft copolymer (A) and the polymer compound (B) obtained by the present production method (or their dried products) can be mixed with the antioxidant described later and the various components described in the item (4-4. Other additives) described later to obtain the modifier for polyacetal resin.

[0125] The modifier obtained by the above-mentioned manufacturing method can be a powder or granular body. In other words, the present modifier can be a powder or granular body. In this specification, "powder or granular body" includes both powder and granular body, and refers to a collection of powders, granules, etc. In addition, when specifically distinguished, "granular body" refers to a substance with a volume average particle size of 0.1mm to 10mm, and "powder" refers to a substance with a volume average particle size of 0.01mm to 0.1mm. In addition, the "volume average particle size" less than 10μm can be measured using a dynamic light scattering (DLS: Dynamic Light Scattering) particle size distribution measuring device Nanotrac WaveII-EX150 (manufactured by Microtrac Bell Co., Ltd.), and the "volume average particle size" in the range of 10μm or more can be measured using a laser diffraction particle size distribution measuring device Microtrac MT3000II (manufactured by Microtrac Bell Co., Ltd.). The volume average particle size of the modifier obtained by the present manufacturing method and the present modifier is not particularly limited, for example, 0.01mm to 10mm.

[0126] [4. Polyacetal resin composition]

[0127] The polyacetal resin composition according to one embodiment of the present invention contains the polyacetal resin modifier described in [2. Polyacetal resin modifier] and a polyacetal resin (C).

[0128] In this specification, "polyacetal resin composition" may be referred to as "resin composition" hereinafter. "Polyacetal resin composition of one embodiment of the present invention" may be referred to as "present resin composition" hereinafter. By molding (e.g., injection molding) the present resin composition, a molded body of polyacetal resin can be produced.

[0129] Since the present resin composition has the above-mentioned structure, it has the advantage of less VOC generation. More specifically, since the present resin composition has the above-mentioned structure, it has the advantage of less VOC generation during and after the molding of the resin composition. In addition, since the present resin composition has the above-mentioned structure, it has excellent weather resistance and also has the advantage of being able to provide a molded body with excellent weather resistance. In addition, since the present resin composition has the above-mentioned structure, the toughness of the obtained molded body, the elasticity of the obtained molded body and the moldability of the resin composition are excellent. In addition, since the present resin composition has the above-mentioned structure, it also has the advantage of being able to provide a molded body with excellent impact resistance. In addition, since the present resin composition has the above-mentioned structure, it also has the advantage of being able to take into account the high impact resistance of the excellent molded body at a high level and preventing or reducing the generation of VOC generated during and after the molding of the resin composition. In addition, since the present resin composition has the above-mentioned structure, it also has the advantage of being able to provide a molded body with excellent softness.

[0130] (4-1. Polyacetal resin (C))

[0131] The polyacetal resin (C) refers to a polymer compound having oxymethylene (-CH2O-) as a main constituent unit (for example, a constituent unit accounting for 50 mol% or more in 100 mol% of all constituent units). The polyacetal resin (C) used in one embodiment of the present invention is not particularly limited. The polyacetal resin (C) may be (a) a homopolymer containing only divalent oxymethylene as a constituent unit, or (b) a copolymer containing divalent oxymethylene and divalent oxyalkylene having 2 or more carbon atoms as constituent units.

[0132] The divalent oxyalkylene group preferably has a carbon number of 2 to 6. Examples of the oxyalkylene group having a carbon number of 2 to 6 include an oxyethylene group, an oxypropylene group, and an oxybutylene group.

[0133] When the polyacetal resin (C) is a copolymer, the ratio of the oxyalkylene groups having 2 to 6 carbon atoms in the polyacetal resin (C) is not particularly limited. The molar number of the oxyalkylene groups having 2 to 6 carbon atoms is preferably 0.4 to 15.0 mol%, more preferably 0.4 to 10.0 mol%, and particularly preferably 0.4 to 5.0 mol% in the total 100 mol% of the oxymethylene groups and the oxyalkylene groups having 2 to 6 carbon atoms in the polyacetal resin (C). This configuration has the advantage of being able to achieve both excellent continuous productivity of the polyacetal resin (C) and excellent thermal stability of the polyacetal resin (C).

[0134] There are no particular restrictions on the method for producing the polyacetal resin (C). In order to produce the polyacetal resin (C), three In order to introduce an oxyalkylene group having 2 to 6 carbon atoms into the polyacetal resin (C), cyclic formals and cyclic ethers can be used. Specific examples of cyclic formals include 1,3-dioxolane, 1,3-dioxolane, Specific examples of cyclic ethers include ethylene oxide, propylene oxide, and butylene oxide. In order to introduce ethylene oxide into the polyacetal resin (C), 1,3-dioxolane can be used as the main raw material. In order to introduce propylene oxide into the polyacetal resin (C), 1,3-dioxolane can be used as the main raw material. In order to introduce oxybutylene groups into the polyacetal resin (C), 1,3-dioxepane can be used as the main raw material. It should be noted that in the polyacetal resin (C), the amount of (i) hemiformal terminal groups, (ii) formyl terminal groups, and (iii) terminal groups unstable to heat, acid, and alkali are as small as possible. Here, the hemiformal terminal group is represented by -OCH2OH, and the formyl terminal group is represented by -CHO.

[0135] The melt index of the polyacetal resin (C) is not particularly limited, and is, for example, preferably 0.1 g / 10 min to 120.0 g / 10 min, more preferably 0.5 g / 10 min to 70.0 g / 10 min, further preferably 0.5 g / 10 min to 30.0 g / 10 min, and particularly preferably 0.5 g / 10 min to 20.0 g / 10 min. In this specification, the melt index of the polyacetal resin (C) is a value measured under the conditions of 190° C. and 2.16 kg in accordance with ASTM-D1238.

[0136] The content ratio of the modifier for polyacetal resin in the polyacetal resin composition is not particularly limited. In the polyacetal resin composition, for example, when the total of the modifier for polyacetal resin and the polyacetal resin (C) is set to 100% by mass, it is preferred that the modifier for polyacetal resin is 3% to 80% by mass, and the polyacetal resin (C) is 20% to 97% by mass, more preferably the modifier for polyacetal resin is 5% to 50% by mass, and the polyacetal resin (C) is 50% to 95% by mass, further preferably the modifier for polyacetal resin is 7% to 30% by mass, and the polyacetal resin (C) is 70% to 93% by mass, and particularly preferably the modifier for polyacetal resin is 9% to 25% by mass, and the polyacetal resin (C) is 75% to 91% by mass. This configuration has the advantages of being able to achieve the following three points at a high level: high weather resistance and high impact resistance of the molded product; and prevention or reduction of the generation of VOCs generated during and after molding of the resin composition.

[0137] The mass ratio of the rubber-containing graft copolymer (A) and the polyacetal resin (C) contained in the modifier for polyacetal resin in the polyacetal resin composition (rubber-containing graft copolymer (A) / polyacetal resin (C)) is preferably 3 / 100 or more, more preferably 4 / 100 or more, more preferably 5 / 100 or more, more preferably 7 / 100 or more, more preferably 9 / 100 or more, further preferably 10 / 100 or more, and particularly preferably 11 / 100 or more. The upper limit of the above-mentioned mass ratio is, for example, preferably 50 / 100 or less, more preferably 40 / 100 or less, more preferably 35 / 100 or less, more preferably 30 / 100 or less, more preferably 25 / 100 or less, and particularly preferably 20 / 100 or less. When the above-mentioned mass ratio is 3 / 100 or more, the obtained polyacetal resin composition can provide a molded body having excellent impact resistance. When the above-mentioned mass ratio is 50 / 100 or less, there is an advantage that the extrusion of the obtained polyacetal resin composition becomes easy.

[0138] (4-2. Formaldehyde scavenger)

[0139] The present resin composition preferably further contains a formaldehyde scavenger. When the present resin composition contains a formaldehyde scavenger, the resin composition has the advantage of generating less VOC. More specifically, when the present resin composition contains a formaldehyde scavenger, the resin composition has the advantage of generating less VOC during and after molding.

[0140] The formaldehyde scavenger is not particularly limited. The formaldehyde scavenger is preferably a compound containing a reactive group reactive to formaldehyde. As the reactive group reactive to formaldehyde, there can be mentioned an amide group, a hydrazide group and a hydrazone group. As the compound containing such a reactive group, there can be mentioned a hydrazide compound, a hydrazone of a hydrazine compound, a guanamine compound and a urea compound. The formaldehyde scavenger preferably contains one or more selected from hydrazide compounds, hydrazones of hydrazine compounds, guanamine compounds and urea compounds, and more preferably one or more selected from them. According to this configuration, there is an advantage that the amount of formaldehyde (VOC) generated during and after the molding of the resin composition is less.

[0141] Examples of the hydrazide compound include aliphatic hydrazide compounds and aromatic hydrazide compounds. Examples of the aliphatic dihydrazide include carbodihydrazide, oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid hydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide (1,12-dodecane dicarbohydrazide), 1,18-octadecane dicarbohydrazide, stearic acid hydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, 7,11-octadecadiene-1,18-dicarbohydrazide, and the like.

[0142] Examples of the aromatic dihydrazide compound include isophthalic acid dihydrazide, terephthalic acid dihydrazide, 1,5-naphthalene dicarbohydrazide, 1,8-naphthalene dicarbohydrazide, 2,6-naphthalene dicarbohydrazide, 4,4′-oxybisbenzenesulfonylhydrazide and 1,5-diphenylcarbohydrazide.

[0143] Examples of the hydrazine compound hydrazone include 1,12-bis[2-(1-methylethylidene)hydrazine]-1,12-dodecanedione, 1,12-bis(2-ethylidenehydrazine)-1,12-dodecanedione, 1,12-bis(2-propylenehydrazine)-1,12-dodecanedione, 1,12-bis[2-(1-methylpropylene)hydrazine]-1,12-dodecanedione, 1,12-bis[2-(1-ethylpropylene)hydrazine]-1,12-dodecanedione, 1,10-bis[2-(1-methylethylidene)hydrazine]]-1,10-decanedione, and 1,10-bis(2-propylenehydrazine)-1,10-decanedione. , 1,10-bis(2-propylenehydrazine)-1,10-decanedione, 1,10-bis[2-(1-methylpropylene)hydrazine]-1,10-decanedione, 1,10-bis[2-(1-ethylpropylene)hydrazine]-1,10-decanedione, 1,6-bis[2-(1-methylethylidene)hydrazine]-1,6-hexanedione, 1,6-bis(2-ethylidenehydrazine)-1,6-hexanedione, 1,6-bis(2-propylenehydrazine)-1,6-hexanedione, 1,6-bis[2-(1-methylpropylene)hydrazine]-1,6-hexanedione, 1,6-bis[2-(1-ethylpropylene)hydrazine]-1,6-hexanedione, etc.

[0144] Examples of the guanamine compound include benzoguanamine and N-methylolated benzoguanamine.

[0145] Examples of the urea compound include ethylene urea, dimethylethylene urea, propylene urea, and tetrabutyl urea.

[0146] From the viewpoint of further reducing the amount of VOC generated during and after molding of the obtained resin composition, the formaldehyde scavenger preferably comprises one or more selected from adipic acid hydrazide, dodecanedioic acid dihydrazide, 1,12-bis[2-(1-methylethylene)hydrazino]-1,12-dodecanedione, benzoguanamine and ethylene urea, and more preferably one or more selected from them.

[0147] The content of the formaldehyde scavenger in the present resin composition is not particularly limited. The content of the formaldehyde scavenger in the present resin composition is, for example, preferably an amount of 3.0 μmol or more of the reactive groups in the formaldehyde scavenger relative to the total of 1 g of the modifier for polyacetal resin and the polyacetal resin (C), more preferably an amount of 8.0 μmol or more of the reactive groups in the formaldehyde scavenger relative to the total of 1 g of the modifier for polyacetal resin and the polyacetal resin (C), further preferably an amount of 10.0 μmol or more of the reactive groups in the formaldehyde scavenger relative to the total of 1 g of the modifier for polyacetal resin and the polyacetal resin (C), and particularly preferably an amount of 15.0 μmol or more of the reactive groups in the formaldehyde scavenger relative to the total of 1 g of the modifier for polyacetal resin and the polyacetal resin (C). For the content of the formaldehyde scavenger in the present resin composition, for example, the reactive group in the formaldehyde scavenger is preferably 100 μmol or less, more preferably 80 μmol or less, and particularly preferably 70 μmol or less relative to 1 g of the total of the modifier for polyacetal resin and the polyacetal resin (C). When the content of the formaldehyde scavenger is within the above range, there are the following advantages: the amount of VOC generated during and after molding of the resin composition is further reduced, and the generation of mold contamination from the formaldehyde scavenger can be prevented or reduced.

[0148] (4-3. Antioxidants)

[0149] The present resin composition may contain an antioxidant within a range that does not impair the effects of one embodiment of the present invention. Examples of the antioxidant include hindered phenol-based antioxidants.

[0150] Examples of hindered phenol antioxidants include 2,2'-methylene-bis(4-methyl-6-tert-butylphenol), 4,4'-methylene-bis(2,6-di-tert-butylphenol), 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 3,5-di-tert-butyl-4-hydroxybenzyl dimethylamine, 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid distearyl ester, 3,5-di-tert-butyl 2,6,7-Trioxa-1-phospha-bicyclo[2.2.2]oct-4-yl-methyl-3,5-di-tert-butyl-4-hydroxyhydrocinnamate, 3,5-di-tert-butyl-4-hydroxyphenyl-3,5-distearyl-thiotriazinylamine, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole, 2,6-di-tert-butyl-4-hydroxymethylphenol, 2,4 -Bis-(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid amide), octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], pentaerythritol-tetrakis[3-(3,5- tert-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3,5-dimethyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2'-thiodiethyl-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and the like.

[0151] The present resin composition may contain only one of the above-mentioned antioxidants, or may contain two or more of them in combination.

[0152] (4-4. Other additives)

[0153] The present resin composition may also include any additives and fillers known in the past within the scope of not damaging the purpose of one embodiment of the present invention. As additives and fillers that can be used in one embodiment of the present invention, for example, thermoplastic resins other than polyacetal resins, light stabilizers, ultraviolet absorbers, hindered amine light stabilizers (HALS), heat stabilizers, antistatic agents, carbon fibers, glass fibers, glass flakes, potassium titanate whiskers, dyes, pigments (such as carbon black and titanium oxide, etc.) and the like can be cited. The details of these additives and fillers can be referred to the records of paragraphs

[0113] to

[0124] of Japanese Patent Publication No. 2017-025257. The contents of paragraphs

[0113] to

[0124] of Japanese Patent Publication No. 2017-025257 are incorporated into this specification.

[0154] (4-5. Method for producing polyacetal resin composition)

[0155] The method for producing the present resin composition is not particularly limited. For example, the present resin composition can be obtained by mixing the polyacetal resin modifier of one embodiment of the present invention, the polyacetal resin (C), and, if necessary, a formaldehyde scavenger, an antioxidant, and / or other additives, and melt-kneading the resulting mixture.

[0156] The method for producing the polyacetal resin composition may be as follows:

[0157] A method for producing a polyacetal resin composition, comprising the step of mixing a polyacetal resin modifier obtained by the method for producing a polyacetal resin modifier described in the above-mentioned item [3. Method for producing a polyacetal resin modifier] and a polyacetal resin (C).

[0158] In the method for producing the resin composition, the raw materials can be mixed using a Henschel mixer and a drum mixer. The obtained mixture can be melt-kneaded using a single-screw or twin-screw extruder, a Banbury mixer, a pressure kneader, a mixing roll or other kneading machine. The melt-kneading of the above-mentioned mixture is preferably carried out at a temperature above the melting temperature of the polyacetal resin, specifically at a melting temperature of the polyacetal resin (generally above 180° C.).

[0159] In particular, in the polyacetal resin composition according to one embodiment of the present invention, in order to prevent or reduce secondary aggregation of the polyacetal resin modifier and adjust the average secondary particle size to an appropriate value, the following method can be preferably used.

[0160] As an example of a preferred manufacturing method for preventing or reducing the secondary coagulation of the polyacetal resin modifier in the polyacetal resin composition, the following method can be cited: after mixing the polyacetal resin and the polyacetal resin modifier with a rotary drum, the obtained mixture is extruded by an extruder to form a strand, and then the strand-shaped mixture is cut to form particles. At this time, as an extruder, a twin-screw extruder is preferably used from the aspect of being able to reduce the generation of secondary coagulation compared to a single-screw extruder. Among them, the ratio of the length L (mm) of the screw to the diameter D (mm) of the screw, i.e., L / D, preferably satisfies the relationship of 20<(L / D)<100, and more preferably satisfies 25<(L / D)<70. By making the ratio (L / D) exceed 20, the polyacetal resin modifier is easily micro-dispersed in the polyacetal resin, and the generation of secondary coagulation of the modifier can be more effectively prevented or reduced. In addition, by making the ratio (L / D) less than 100, it is possible to effectively prevent or reduce the resin composition from being easily discolored due to thermal degradation.

[0161] The shape of the die nozzle is not particularly limited, but from the aspect of the particle shape, a circular nozzle with a diameter of 1 mm to 10 mm is preferred, and a circular nozzle with a diameter of 2 mm to 7 mm is more preferred. The circular shape here is not limited to a circle in a geometric sense, but is intended to be interpreted as a substantially circular shape in the technical field of one embodiment of the present invention.

[0162] In addition, the melting temperature of the resin composition during melt kneading is appropriately determined according to the relationship with the melting temperature of the resin. In this specification, the above-mentioned melting temperature is a measured temperature obtained by measuring the resin coming out of the die hole (die nozzle) of the extruder using a thermocouple. The above-mentioned melting temperature is preferably above 170°C, more preferably above 180°C, and further preferably above 190°C. In addition, the above-mentioned melting temperature is preferably below 250°C, more preferably below 230°C. By making the above-mentioned melting temperature above 170°C, there is a tendency that melting is fully carried out and production volume is significantly improved. In addition, by making the above-mentioned melting temperature below 250°C, discoloration of the resin composition caused by thermal degradation can be more effectively prevented or reduced.

[0163] The screw speed during melt kneading is preferably 50 rpm to 500 rpm, and more preferably 70 rpm to 350 rpm. By making the screw speed above 50 rpm, the modifier for polyacetal resin is easily microdispersed in the polyacetal resin, and the secondary agglomeration of the modifier can be more effectively prevented or reduced. In addition, by being below 500 rpm, the heat generated during melt kneading can be significantly prevented or reduced, and the discoloration of the resin composition caused by thermal degradation can be effectively prevented or reduced. In addition, the discharge amount of the mixture from the die hole is preferably 5 kg / hr to 1000 kg / hr, and more preferably 7 kg / hr to 800 kg / hr. By making the above discharge amount above 5 kg / hr, the modifier for polyacetal resin is easily microdispersed, and the secondary agglomeration can be effectively prevented or reduced. In addition, by making the above discharge amount below 1000 kg / hr, the heat generated during melt kneading can be effectively prevented or reduced, and the discoloration of the resin composition caused by thermal degradation can be more effectively prevented or reduced.

[0164] 〔5. Application〕

[0165] The present modifier and the present resin composition can be appropriately used for various purposes such as electrical and electronic applications, vehicle applications, industrial equipment applications, etc. For example, the present modifier and the present resin composition can be appropriately used for mechanical parts of the drive part of AV equipment, handles of dishwashing and drying machines, speaker grilles, propellers for stirring sinks, switches of OA equipment, gears, automotive wiper motor system gears, regulator handles, interior door handles, door lock side housings, gear shift levers, heater fans, pipe brackets, power window regulators, seat belt related parts, power seat gears, sunroofs, clamps, fasteners, screws of industrial equipment conveyors, belt conveyors, chains, torque limiters, etc.

[0166] One embodiment of the present invention may be configured as follows.

[0167] [1] A modifier for a polyacetal resin, comprising a rubber-containing graft copolymer (A) and a polymer compound (B) having a glycidyl group, wherein the rubber-containing graft copolymer (A) comprises an elastomer and a graft portion graft-bonded to the elastomer, the graft portion being composed only of constituent units derived from a vinyl monomer having no reactive functional group, the mass ratio of the elastomer to the graft portion (parts by mass of the elastomer / parts by mass of the graft portion) being 60 / 40 to 95 / 5, the content of chlorine in the modifier for polyacetal resin being 1 ppm to 170 ppm based on the mass of the modifier for polyacetal resin, the content of calcium in the modifier for polyacetal resin being 1 ppm to 780 ppm based on the mass of the modifier for polyacetal resin, and the pH of a mixture of 10 parts by mass of the modifier for polyacetal resin and 100 parts by mass of deionized water being 6.0 to 8.0.

[0168] [2] The polyacetal resin modifier according to [1], wherein the polymer compound (B) is at least one of epoxidized soybean oil and epoxidized castor oil.

[0169] [3] The polyacetal resin modifier according to [1] or [2], wherein the elastomer is composed only of (meth)acrylate rubber.

[0170] [4] The polyacetal resin modifier according to any one of [1] to [3], wherein the epoxy group content of the polyacetal resin modifier is 15 μmol / g to 180 μmol / g.

[0171] [5] The polyacetal resin modifier according to any one of [1] to [4], wherein the content of the polymer compound (B) in the polyacetal resin modifier is 0.1 to 5.0 parts by mass relative to 100 parts by mass of the rubber-containing graft copolymer (A).

[0172] [6] The polyacetal resin modifier according to any one of [1] to [5], wherein the polyacetal resin modifier is a powder or granular material.

[0173] [7] A polyacetal resin composition comprising the polyacetal resin modifier according to any one of [1] to [6] and a polyacetal resin (C).

[0174] [8] The polyacetal resin composition according to [7], wherein, when the total of the polyacetal resin modifier and the polyacetal resin (C) is 100 mass %, the polyacetal resin modifier is 3 mass % to 80 mass %, and the polyacetal resin (C) is 20 mass % to 97 mass %.

[0175] [9] The polyacetal resin composition according to [7] or [8], further comprising a formaldehyde scavenger.

[0176]

[10] A polyacetal resin composition according to [9], wherein the formaldehyde scavenger comprises a reactive group reactive to formaldehyde, and the content of the formaldehyde scavenger in the polyacetal resin composition is an amount of 3.0 μmol or more relative to 1 g of the total of the modifier for the polyacetal resin and the polyacetal resin (C).

[0177]

[11] The polyacetal resin composition according to [9] or

[10] , wherein the formaldehyde scavenger comprises one or more selected from the group consisting of hydrazide compounds, hydrazone compounds, guanamine compounds, and urea compounds.

[0178]

[12] A method for producing a modifier for polyacetal resin, comprising: a polymer compound (B) adding step, wherein a polymer compound (B) having a glycidyl group is added in an emulsified state to an aqueous latex containing a rubber-containing graft copolymer (A); a coagulation step, wherein calcium chloride is added to the aqueous latex obtained in the polymer compound (B) adding step to obtain a coagulation body containing the rubber-containing graft copolymer (A) and the polymer compound (B); and a washing step, wherein the coagulation body obtained in the coagulation step is washed, wherein the rubber-containing graft copolymer (A) has an elastomer and a graft portion graft-bonded to the elastomer, the graft portion being composed only of constituent units derived from a vinyl monomer having no reactive functional group, the mass ratio of the elastomer to the graft portion (mass part of the elastomer / mass part of the graft portion) is 60 / 40 to 95 / 5, and the pH of the aqueous latex is 5 to 9.

[0179]

[13] The method for producing a polyacetal resin modifier according to

[12] , wherein the polymer compound (B) is at least one of epoxidized soybean oil and epoxidized castor oil.

[0180]

[14] The method for producing a polyacetal resin modifier according to

[12] or

[13] , wherein the elastomer is composed only of (meth)acrylate rubber.

[0181]

[15] The method for producing a polyacetal resin modifier according to any one of

[12] to

[14] , wherein the epoxy group content in the polyacetal resin modifier is 15 μmol / g to 180 μmol / g.

[0182]

[16] A method for producing a modifier for a polyacetal resin according to any one of

[12] to

[15] , wherein the content of the polymer compound (B) in the modifier for the polyacetal resin is 0.1 to 5.0 parts by mass relative to 100 parts by mass of the rubber-containing graft copolymer (A).

[0183]

[17] The method for producing a polyacetal resin modifier according to any one of

[12] to

[16] , wherein the polyacetal resin modifier is in the form of a powder or granular material.

[0184]

[18] A method for producing a polyacetal resin composition, comprising the step of mixing a polyacetal resin modifier obtained by the method for producing a polyacetal resin modifier according to any one of

[12] to

[17] and a polyacetal resin (C).

[0185]

[19] A method for producing a polyacetal resin composition according to

[18] , wherein, when the total of the polyacetal resin modifier and the polyacetal resin (C) is set to 100 mass%, the polyacetal resin modifier is 3 mass% to 80 mass%, and the polyacetal resin (C) is 20 mass% to 97 mass%.

[0186]

[20] The method for producing a polyacetal resin composition according to

[18] or

[19] , further comprising a formaldehyde scavenger.

[0187]

[21] A method for producing a polyacetal resin composition according to

[20] , wherein the formaldehyde scavenger comprises a reactive group reactive to formaldehyde, and the content of the formaldehyde scavenger in the polyacetal resin composition is an amount of 3.0 μmol or more relative to 1 g of the total of the modifier for the polyacetal resin and the polyacetal resin (C).

[0188]

[22] The method for producing a polyacetal resin composition according to

[20] or

[21] , wherein the formaldehyde scavenger comprises one or more selected from the group consisting of hydrazide compounds, hydrazine compound hydrazones, guanamine compounds, and urea compounds.

[0189] Example

[0190] Hereinafter, an embodiment of the present invention will be described in more detail by examples and comparative examples, but the present invention is not limited to these examples. An embodiment of the present invention can be implemented by appropriately changing within the scope of the above or later-described subject matter, and these changed embodiments are all included in the technical scope of the present invention. It should be noted that in the following examples and comparative examples, "parts" and "%" refer to "parts by mass" or "mass %" respectively.

[0191] <Ingredients>

[0192] The components used in each of the preparation examples, examples and comparative examples are as follows.

[0193] Rubber-containing graft copolymer (A)

[0194] The rubber-containing graft copolymer obtained in the following Production Examples was used.

[0195] ·Polymer compound having a glycidyl group (B)

[0196] Epoxidized soybean oil (O-130P manufactured by ADEKA)

[0197] Coagulant

[0198] Calcium chloride dihydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0199] Polyacetal resin (C)

[0200] The polyacetal resin obtained in the following production example was used.

[0201] Formaldehyde scavenger

[0202] (D-1): Ethylene urea (manufactured by Kanto Chemical Co., Ltd.)

[0203] (D-2): 1,12-bis[2-(1-methylethylidene)hydrazino]]-1,12-dodecanedione (manufactured by Japan Finechem Co., Ltd.)

[0204] (D-3): Adipic acid dihydrazide (manufactured by Japan Finechem Co., Ltd.)

[0205] (D-4): Dodecanedioic acid dihydrazide (manufactured by Japan Finechem Co., Ltd.)

[0206] (D-5): Benzoguanamine (manufactured by Nippon Chemical Co., Ltd.)

[0207] Antioxidants

[0208] IRGANOX245 (manufactured by BASF)

[0209] DLTP "Yoshitomi" (manufactured by API Corporation)

[0210] UV absorber

[0211] Tinuvin 234 (manufactured by BASF)

[0212] HALS

[0213] Tinvin 622SF (manufactured by BASF).

[0214] <Measurement method>

[0215] The measurement methods in Examples and Comparative Examples are described below.

[0216] (Measurement method of volume average particle size)

[0217] The volume average particle size (Mv) of the elastomer or rubber-containing graft copolymer (A) dispersed in the aqueous latex is measured using Nanotrac WaveII-EX150 (manufactured by Microtrac Bell Co., Ltd.). The substance obtained by diluting the aqueous latex with deionized water is used as the measurement sample. The measurement is carried out as follows: the refractive index of the elastomer or polymer microparticles (A) obtained in each manufacturing example and the water is input, and the sample concentration is adjusted in a manner such that the measurement time is 120 seconds and the load index is within the range of 1 to 10.

[0218] (Method for measuring the conductivity of cleaning water)

[0219] The cleaning water was used as a sample and the conductivity of the cleaning water was measured using ES-71 manufactured by HORIBA.

[0220] (Method for determining the content of chlorine and calcium in modifier)

[0221] 4.0 g of the modifier obtained in each example and comparative example was measured. The amount of chlorine and calcium elements in the modifier was measured using the energy dispersive fluorescent X-ray device "SPECTRO XEPOS" manufactured by Rigaku Corporation. The results obtained are expressed as the mass % of each element relative to 100 mass % of the modifier. In addition, the results are not shown for the element content of less than 0.001%. It can be said that the element content in the modifier is less than 0.001% (i.e., less than 10 ppm) does not affect the effect of one embodiment of the present invention.

[0222] (Method for determining pH of a mixture of a modifier and deionized water)

[0223] 10 parts by mass of the modifier obtained in each of the examples and comparative examples and 100 parts by mass of deionized water were mixed to obtain a mixture, and the obtained mixture was stirred for 30 minutes. The pH of the obtained mixture (25° C.) was measured using a pH meter.

[0224] (Method for determining the epoxy group content in the modifier)

[0225] The modifier obtained in each example and comparative example was added to deuterated chloroform containing 1,4-bis(trimethylsilyl)benzene-d4 (hereinafter referred to as BTMSB-d4) as an internal standard, and the obtained mixed solution was stirred to disperse the modifier in the deuterated chloroform. After the obtained dispersion was allowed to stand, the lower layer was collected and filtered using a PTFE filter with a pore size of 0.2 μm to obtain a filtrate. The filtrate was used as a sample and subjected to AVANCE NEO 700 manufactured by Bruker. 1 H NMR measurement. The epoxy content in the modifier was determined from the ratio of the peak area of ​​the trimethylsilyl group (0.3 ppm) of BTMSB-d4 with a known concentration of 0.71 mg / ml to the peak area of ​​the characteristic glycerol part (4.3 ppm) of the epoxidized soybean oil as the polymer compound (B). It should be noted that, as shown in the following description, the compound containing an epoxy group in the materials used in each example and comparative example is only the polymer compound (B).

[0226] (Method for manufacturing ISO test piece)

[0227] The pellets of the polyacetal resin composition obtained in each embodiment and comparative example were injection molded using an injection molding machine EC-100 manufactured by Toshiba Machinery in accordance with ISO9988-2 standard. Here, the barrel temperature was set to 195°C and the mold temperature was set to 90°C. By this injection molding, a multi-purpose test piece (as an ISO test piece) with a thickness of 4 mm was obtained. Using the obtained ISO test piece, the Charpy impact value and bending modulus of the notched zone were measured. It should be noted that the ISO test piece can also be said to be a molded body of the polyacetal resin composition.

[0228] (Evaluation method of weather resistance)

[0229] The ISO test piece obtained in the above (method for producing an ISO test piece) was tested using S80 manufactured by Suga Test Instrument Co., Ltd. under the conditions of a sunlight carbon arc lamp (light source), 83°C (black panel temperature), no rain, #255 (filter), 50% OH (humidity) and 255 W / m 2The weather resistance test is carried out under a test environment of (300 to 700 nm) (radiant illuminance) to evaluate the crack generation time at this time. It should be noted that from a practical point of view, if the crack generation time of the ISO test piece of the polyacetal resin composition is 150 hours or more, it can be judged that the polyacetal resin composition has excellent weather resistance and can provide a molded body with excellent weather resistance.

[0230] In addition, in applications requiring weather resistance, UV absorbers and / or hindered amine light stabilizers (HALS) are generally added to polyacetal resins. In the examples, polyacetal resin compositions to which UV absorbers and hindered amine light stabilizers are added are also used to prepare ISO test pieces for evaluating weather resistance.

[0231] (Measurement method of impact resistance)

[0232] Using a notching tool manufactured by Toyo Seiki Co., Ltd., a test piece of 80 mm in length × 10 mm in width × 4 mm in thickness was cut from the ISO test piece, and a notch with a front end radius of r = 0.25 mm was processed on the test piece. Then, the obtained test piece was subjected to a Charpy impact test according to ISO179-1 at room temperature (23°C) to obtain the notched Charpy impact value. It should be noted that from a practical point of view, if the notched Charpy impact value of the test piece of the polyacetal resin composition is 10 kj / m 2 In addition, from a comparative point of view, if the ratio of the notched Charpy impact value of the test piece of the polyacetal resin composition containing the modifier to the notched Charpy impact value measured in the test piece of the polyacetal resin alone (i.e., Reference Example 1) contained in the polyacetal resin composition (notched Charpy impact value of the test piece of the polyacetal resin composition containing the modifier / notched Charpy impact value of the test piece of the polyacetal resin alone (i.e., Reference Example 1)) is 1.1 or more, it can be judged that the polyacetal resin composition can provide a molded body with excellent impact resistance.

[0233] (Measurement method of flexural elastic modulus)

[0234] The ISO test piece is used as a sample, and a fully automatic bending tester is used as a bending tester. The bending test is performed at a bending test speed of 2 mm / minute according to the method described in ISO178 to determine the bending elastic modulus. It should be noted that from a practical point of view, if the bending elastic modulus of the ISO test piece of the polyacetal resin composition is less than 2300 MPa, it can be judged that the polyacetal resin composition can provide a molded body with excellent softness. In addition, from a comparative point of view, if the bending elastic modulus of the ISO test piece of the polyacetal resin composition containing a modifier is relative to the ratio of the bending elastic modulus measured in the ISO test piece of the polyacetal resin alone (i.e., Reference Example 1) contained in the polyacetal resin composition (bending elastic modulus of the ISO test piece of the polyacetal resin composition containing a modifier / bending elastic modulus of the ISO test piece of the polyacetal resin alone (i.e., Reference Example 1)) is less than 0.9, it can be judged that the polyacetal resin composition can provide a molded body with excellent softness.

[0235] (Method for preparing flat test piece)

[0236] The pellets of the polyacetal resin composition obtained in each example and comparative example were heat treated in a hot air circulation dryer at a temperature of 80°C for 4 hours. Next, the heat-treated pellets were injection molded using an injection molding machine SE-30 manufactured by Sumitomo Heavy Industries, Ltd. at a barrel temperature of 215°C and a mold temperature of 80°C to produce a 100 mm × 40 mm × 2 mm flat test piece. It should be noted that the flat test piece can also be said to be a molded body of the polyacetal resin composition.

[0237] (Method for measuring the amount of formaldehyde generated)

[0238] On the second day after the flat test piece was prepared, the flat test piece was used to measure the formaldehyde generation amount (μg / g-POM, which means the formaldehyde generation amount (μg) per 1g of polyacetal resin) according to the method described in the German automotive industry joint standard VDA275 (Automotive interior parts-Quantification of formaldehyde emission based on the revised flask method). The specific measurement method is as follows.

[0239] (1) 50 mL of distilled water was placed in a polyethylene container, the flat test piece was placed in the polyethylene container in a suspended state, the polyethylene container was covered, and the polyethylene container was heated at 60° C. for 3 hours in a sealed state.

[0240] (2) Next, the polyethylene container was left to stand at room temperature for 60 minutes, and then the flat test piece was taken out from the polyethylene container.

[0241] (3) The distilled water was used as a sample, and the amount of formaldehyde absorbed in the distilled water in the polyethylene container was measured by the acetylacetone colorimetric method using a UV spectrometer. The value obtained by dividing the obtained amount of formaldehyde by the mass of the polyacetal resin (C) in the flat test piece was taken as the amount of formaldehyde generated in the flat test piece.

[0242] It should be noted that, from a practical point of view, if the formaldehyde generation amount of the flat test piece of the polyacetal resin composition is 20.0 μg / g-POM or less, it can be judged that the VOC generation amount of the polyacetal resin composition during and after molding is small. In addition, from a comparative point of view, if the ratio of the formaldehyde generation amount of the flat test piece of the polyacetal resin composition containing the modifier to the formaldehyde generation amount measured in the flat test piece of the polyacetal resin alone (i.e., Reference Example 1) contained in the polyacetal resin composition (formaldehyde generation amount of the flat test piece of the polyacetal resin composition containing the modifier / formaldehyde generation amount of the flat test piece of the polyacetal resin alone (i.e., Reference Example 1)) is 2.0 or less, it can be judged that the formaldehyde generation amount (VOC generation amount) of the polyacetal resin composition during and after molding is small.

[0243] Furthermore, in areas where the amount of formaldehyde generated is strictly restricted, such as automotive interior applications, the amount of formaldehyde generated can be further suppressed by using a formaldehyde scavenger. When a polyacetal resin composition contains a formaldehyde scavenger (e.g., a formaldehyde scavenger containing a reactive group in an amount of 8.9 μmol or more relative to 1 g of the total of the modifier for polyacetal resin and the polyacetal resin (C)), if the formaldehyde generation of a flat plate test piece of the polyacetal resin composition is 2.5 μg / g-POM or less, it can be determined that the polyacetal resin composition has a low amount of VOC generated during and after molding. In addition, from a comparative point of view, if the ratio of the formaldehyde generation amount of the flat plate test piece of the polyacetal resin composition containing the modifier to the formaldehyde generation amount measured in the flat plate test piece of the polyacetal resin alone (i.e., Reference Example 2) contained in the polyacetal resin composition (formaldehyde generation amount of the flat plate test piece of the polyacetal resin composition containing the modifier / formaldehyde generation amount of the flat plate test piece of the polyacetal resin alone (i.e., Reference Example 2)) is 2.5 or less, it can be judged that the formaldehyde generation amount (VOC generation amount) of the polyacetal resin composition during and after molding is small.

[0244] Next, each manufacturing method, each example, and each comparative example are described below.

[0245] <Preparation of Rubber-Containing Graft Copolymer (A)>

[0246] [Production Example 1] Synthesis of aqueous latex containing rubber-containing graft copolymer (A)

[0247] While blowing nitrogen into a pressure-resistant polymerizer equipped with a stirrer, 100 parts of pure water and 0.014 parts of sodium polyoxyethylene alkyl ether phosphate as a surfactant are added. Next, while stirring the raw materials added, the gas inside the pressure-resistant polymerizer is replaced with nitrogen, thereby fully removing the oxygen inside the pressure-resistant polymerizer. Then, the temperature of the solution in the pressure container is raised to 50°C. Then, 8.5 parts of butyl acrylate (BA), 0.04 parts of allyl methacrylate and 0.002 parts of tert-butyl hydroperoxide (BHP) are added to the pressure container at one time. Then, 0.002 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.0012 parts of ferrous sulfate and 0.05 parts of sodium formaldehyde sulfoxylate (SFS) are added to the pressure container. Then, polymerization is carried out for 1 hour. Then, a mixture of 0.68 parts of sodium polyoxyethylene alkyl ether phosphate, 64.5 parts of BA, 0.32 parts of allyl methacrylate and 0.02 parts of BHP as a surfactant was added to the pressure vessel over 210 minutes. Then, the reaction solution in the pressure polymerizer was kept at 50°C for 45 minutes to polymerize to obtain an aqueous latex containing an elastomer. Next, 73 parts of solid components of the elastomer (50°C) and 150 parts of pure water (50°C) were added to the glass reactor. Here, the glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen gas inlet and a monomer addition device. While replacing the gas in the glass reactor with nitrogen, the raw materials added were stirred at 50°C. Next, a mixture of 25.3 parts of methyl methacrylate (MMA) and 1.7 parts of BA as monomer components was added to the glass reactor over 1 hour. While adding the above-mentioned monomer components (i.e., MMA and BA), 0.0125 parts of BHP were added to the glass reactor. After the addition of BHP was completed, the temperature of the reaction solution in the glass reactor was maintained at 50°C for 1 hour to carry out polymerization, thereby obtaining an aqueous latex containing a rubber-containing graft copolymer (A). The volume average particle size of the rubber-containing graft copolymer (A) contained in the obtained aqueous latex was 200 nm.

[0248] <Preparation of emulsion of polymer compound (B)>

[0249] Using a homomixer HM-310 (manufactured by AS ONE), 4.5 parts by mass of pure water, 0.45 parts by mass of sodium polyoxyethylene alkyl ether phosphate as an emulsifier, 1 part by mass of epoxidized soybean oil as a polymer compound (B), 0.125 parts by mass of IRGANOX 245, and 0.375 parts by mass of DLTP "Yoshitomi" were stirred at 10000 rpm for 10 minutes. By this operation, an emulsion of epoxidized soybean oil as a polymer compound (B) having a glycidyl group was obtained.

[0250] <Preparation of Modifier for Polyacetal Resin>

[0251] (Example 1)

[0252] To an aqueous latex containing 100 parts by mass of a solid content of a rubber-containing graft copolymer (A), 6.45 parts by mass of an emulsion of a polymer compound (B) corresponding to 1 part by mass of epoxidized soybean oil as a polymer compound (B) are added. Then, an aqueous solution of calcium chloride is added to the obtained aqueous latex to perform coagulation, thereby obtaining a slurry containing a coacervate containing the rubber-containing graft copolymer (A) and the polymer compound (B). The amount of calcium chloride used is 3.5 parts by mass relative to 100 parts by mass of the total amount of the rubber-containing graft copolymer (A) and the polymer compound (B). Next, the obtained slurry is dehydrated to recover the coacervate. Next, the coacervate is washed with 1000 parts by mass of washing water relative to 100 parts by mass of the solid content of the coacervate, and the coacervate is further dehydrated. Then, the obtained coacervate is dried to obtain a modifier (M-1) for polyacetal resin containing a rubber-containing graft copolymer (A) and a polymer compound (B). The contents of chlorine and calcium elements and pH of the obtained modifier were measured. The results are shown in Table 1.

[0253] (Examples 2 to 4, Comparative Examples 1 and 2)

[0254] In Examples 2 to 4 and Comparative Examples 1 and 2, the amount of the emulsion of the polymer compound (B) having a glycidyl group (i.e., the amount of epoxidized soybean oil as the polymer compound (B)) and the amount of washing water used were changed as shown in Table 1, and the modifier for polyacetal resin was prepared by the same operation as in Example 1. That is, in Comparative Example 1, the polymer compound (B) having a glycidyl group was not used, and in Comparative Example 2, the obtained agglomerates were not washed. In addition, the modifiers obtained in Examples 2 to 4 and Comparative Examples 1 and 2 were respectively designated as modifiers (M-2) to (M-6). The contents of chlorine and calcium elements and pH of each of the obtained modifiers were measured, and the results are shown in Table 1.

[0255] (Comparative Example 3)

[0256] An aqueous latex containing 100 parts by weight of solid content of a rubber-containing graft copolymer (A) is placed in a container, and the water in the container is evaporated using a vacuum pump with a cold trap, thereby obtaining a slurry containing a coagulation containing the rubber-containing graft copolymer (A). Next, the coagulation is washed with 2500 parts of pure water relative to 100 parts of the solid content of the coagulation as washing water, and the coagulation is further dehydrated. Then, the obtained coagulation is dried to obtain a modifier (M-7) for polyacetal resin containing a rubber-containing graft copolymer (A). The element contents of chlorine and calcium and the pH of the obtained modifier are measured, and the results are shown in Table 1. It should be noted that "ND" is the abbreviation of Not Detection, which means that an element cannot be detected (undetectable).

[0257] (Comparative Example 4)

[0258] To an aqueous latex containing 100 parts by mass of a solid content of a rubber-containing graft copolymer (A), 19.35 parts by mass of an emulsion of a polymer compound (B) equivalent to 3 parts by mass of epoxidized soybean oil as a polymer compound (B) was added. Then, 3.5 parts by mass of an aqueous solution of magnesium chloride as a coagulant was added to the obtained aqueous latex to perform coagulation, thereby obtaining a slurry containing a coagulant containing the rubber-containing graft copolymer (A) and the polymer compound (B). Next, the obtained slurry was dehydrated to recover the coagulant. Next, the coagulant was washed with 2500 parts by mass of washing water relative to 100 parts by mass of the solid content of the coagulant, and the coagulant was further dehydrated. Then, the obtained coagulant was dried to obtain a modifier (M-8) for polyacetal resin containing a rubber-containing graft copolymer (A) and a polymer compound (B). The contents of chlorine and calcium elements and pH of the obtained modifier were measured, and the results are shown in Table 1. It should be noted that "ND" is an abbreviation of Not Detection, which means that an element cannot be detected (cannot be detected).

[0259] (Comparative Example 13)

[0260] <Preparation of a modifier for polyacetal resin (M-9) comprising a rubber-containing graft copolymer containing a structural unit derived from a vinyl monomer having a reactive functional group>

[0261] <Synthesis of a rubber-containing graft copolymer comprising a structural unit derived from a vinyl monomer having a reactive functional group>

[0262] While blowing nitrogen into a pressure-resistant polymerizer equipped with a stirrer, 100 parts of pure water and 0.014 parts of sodium polyoxyethylene alkyl ether phosphate as a surfactant are added. Next, while stirring the raw materials, the gas inside the pressure-resistant polymerizer is replaced with nitrogen, thereby fully removing the oxygen inside the pressure-resistant polymerizer. Then, the temperature of the solution in the pressure container is raised to 50°C. Then, 8.5 parts of butyl acrylate (BA), 0.04 parts of allyl methacrylate and 0.002 parts of tert-butyl hydroperoxide (BHP) are added to the pressure container at one time. Then, 0.002 parts of disodium ethylenediaminetetraacetic acid (EDTA), 0.0012 parts of ferrous sulfate and 0.05 parts of sodium formaldehyde sulfoxylate (SFS) are added to the pressure container. Then, polymerization is carried out for 1 hour. Then, a mixture of 0.68 parts of sodium polyoxyethylene alkyl ether phosphate, 44.5 parts of BA, 0.32 parts of allyl methacrylate and 0.02 parts of BHP as a surfactant was added to the pressure vessel over 210 minutes. Then, the reaction solution in the pressure polymerizer was kept at 50°C for 45 minutes to polymerize to obtain an aqueous latex containing an elastomer. Next, 73 parts of the solid content of the elastomer (50°C) and 150 parts of pure water (50°C) were added to the glass reactor. Here, the glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen gas inlet and a monomer addition device. While replacing the gas in the glass reactor with nitrogen, the raw materials added were stirred at 50°C. Next, a mixture of 20.3 parts of methyl methacrylate (MMA), 5 parts of glycidyl methacrylate (GMA) and 1.7 parts of BA as monomer components was added to the glass reactor over 1 hour. While adding the above-mentioned monomer components (i.e., MMA, GMA, and BA), 0.0125 parts of BHP were added to the glass reactor. After the addition of BHP was completed, the temperature of the reaction solution in the glass reactor was maintained at 50° C. for 1 hour to perform polymerization, thereby obtaining an aqueous latex containing a rubber-containing graft copolymer containing a constituent unit derived from a vinyl monomer having a reactive functional group. The volume average particle size of the rubber-containing graft copolymer containing a constituent unit derived from a vinyl monomer having a reactive functional group contained in the obtained aqueous latex was 200 nm.

[0263] Then, an aqueous solution of calcium chloride is added to the obtained aqueous latex to perform coagulation, thereby obtaining a slurry containing a coagulation of a rubber-containing graft copolymer containing a constituent unit derived from a vinyl monomer having a reactive functional group. The amount of calcium chloride used is 3.5 parts by mass relative to 100 parts by mass of the above-mentioned rubber-containing graft copolymer. Then, the obtained slurry is dehydrated to recover the coagulation. Then, the coagulation is washed with 1000 parts by mass of washing water relative to 100 parts by mass of the solid content of the coagulation, and the coagulation is further dehydrated. Then, the obtained coagulation is dried to obtain a modifier (M-9) for polyacetal resin containing a rubber-containing graft copolymer containing a constituent unit derived from a vinyl monomer having a reactive functional group. The contents of chlorine and calcium elements and pH of the obtained modifier are measured, and the results are shown in Table 1.

[0264] In all Examples and Comparative Examples 1, 2, 4, and 13, pure water having an electrical conductivity of 0.1 mS / m was used as the washing water.

[0265] [Table 1]

[0266]

[0267] <Preparation of polyacetal resin>

[0268] [Production Example 2] Synthesis of polyacetal resin (C)

[0269] Make three Alkane and 1,3-dioxolane are copolymerized in such a manner that the content of the constituent unit derived from 1,3-dioxolane in 100% by mass of the obtained polyacetal resin becomes 3.8% by mass (4.6 mol%). 0.3 parts by mass of IRGANOX245 and 0.05 parts by mass of melamine are added to the obtained copolymer. The obtained mixture is melt-kneaded at 222°C for 20 minutes, and the obtained resin is used as a polyacetal resin (C). The melt index (ASTM-D1238 standard: 190°C, 2.16kg) of the obtained polyacetal resin (C) is 10.5g / 10 minutes.

[0270] (Examples 5 to 11, Comparative Examples 5 to 8, 14 and Reference Example 1)

[0271] (Production of polyacetal resin composition)

[0272] Each of the modifiers for polyacetal resin composition (M1 to M9) and the polyacetal resin (C) were dry-blended in the blending ratios shown in Tables 2 and 3. Next, the obtained mixture was melt-shear-mixed using a twin-screw extruder with a screw diameter (D) of 30 mm, a screw length (L) of 760 mm, and a die nozzle diameter of 3.5 mm ("PCM-30" manufactured by Ikegai Co., Ltd.) at a barrel temperature (melting temperature) of 200°C, a screw rotation speed of 120 rpm, and a discharge rate of 10 kg / hour to produce pellets of the polyacetal resin composition.

[0273] Next, the obtained pellets (polyacetal resin composition) were dried at 90°C for 5 hours. Then, the dried pellets of the polyacetal resin composition were injection molded using an injection molding machine EC-100 manufactured by Toshiba Machine at a barrel temperature of 195°C and a mold temperature of 90°C to produce ISO test pieces. The obtained ISO test pieces were used to measure the impact resistance and bending modulus. In addition, the obtained pellets (polyacetal resin composition) were used to make flat test pieces by the above method, and the formaldehyde generation was measured using the flat test pieces. These results are shown in Tables 2 and 3.

[0274] In Comparative Example 14 using the modifier for polyacetal resin composition (M-9), a large amount of agglomerates were observed on the surface of the obtained polyacetal resin composition pellets, so ISO test pieces and flat plate test pieces were not prepared and evaluated. Table 2 states that "no test piece was prepared".

[0275] (Examples 12 to 24, Comparative Examples 9 to 12 and Reference Example 2)

[0276] (Production of polyacetal resin composition)

[0277] Each of the modifiers (M1 to M8) for polyacetal resin composition, polyacetal resin (C) and formaldehyde scavenger were dry-blended in the proportions shown in Tables 4 and 5. In each of the examples and comparative examples, each of the substances shown in Tables 4 and 5 was used as the formaldehyde scavenger. Next, a twin-screw extruder with a vent having a screw diameter (D) of 30 mm, a screw length (L) of 760 mm, and a die nozzle diameter of 3.5 mm ("PCM-30" manufactured by Ikegai Co., Ltd.) was used to melt-shear-mix the obtained mixture at a barrel temperature (melting temperature) of 200°C, a screw speed of 120 rpm, and a discharge rate of 10 kg / hour to produce pellets of the polyacetal resin composition.

[0278] Next, the obtained pellets (polyacetal resin composition) were dried at 90°C for 5 hours. Then, the dried pellets of the polyacetal resin composition were injection molded using an injection molding machine EC-100 manufactured by Toshiba Machine at a barrel temperature of 195°C and a mold temperature of 90°C to produce ISO test pieces. The obtained ISO test pieces were used to measure the impact resistance and bending modulus. In addition, the obtained pellets (polyacetal resin composition) were used to make flat test pieces by the above method, and the formaldehyde generation was measured using the flat test pieces. These results are shown in Tables 4 and 5.

[0279] (Examples 25 to 30, Comparative Example 15)

[0280] (Production of polyacetal resin composition)

[0281] Each of the modifiers for polyacetal resin composition (M1 to M4, M10), polyacetal resin (C), 0.4 parts by weight of Tinuvin 234 and 0.3 parts by weight of Tinuvin 622 were dry-blended. Then, the obtained mixture was melt-shear-mixed at a barrel temperature (melting temperature) of 200°C, a screw speed of 120 rpm and a discharge rate of 10 kg / hour using a twin-screw extruder ("PCM-30" manufactured by Ikegai Co., Ltd.) with a vent having a screw diameter (D) of 30 mm, a screw length (L) of 760 mm and a die nozzle diameter of 3.5 mm, to produce pellets of the polyacetal resin composition. It should be noted that in Comparative Example 15, Kanes M-910 manufactured by Kaneka Co., Ltd., which is a graft copolymer containing butadiene-based rubber, was used as the modifier M-10.

[0282] Next, the obtained pellets (polyacetal resin composition) were dried at 90°C for 5 hours. Then, the pellets of the dried polyacetal resin composition were injection molded at a barrel temperature of 195°C and a mold temperature of 90°C using an injection molding machine EC-100 manufactured by Toshiba Machinery to prepare ISO test pieces. The obtained ISO test pieces were used to measure impact resistance, bending modulus and weather resistance. In addition, the obtained pellets (polyacetal resin composition) were used to prepare flat plate test pieces by the above method, and the formaldehyde generation was measured using the flat plate test pieces. These results are shown in Table 6.

[0283] [Table 2]

[0284]

[0285] [Table 3]

[0286]

[0287] [Table 4]

[0288]

[0289] [Table 5]

[0290]

[0291] [Table 6]

[0292]

[0293] As shown in Tables 2 to 5, it can be seen that the modifier for polyacetal resin according to one embodiment of the present invention can provide a polyacetal resin composition that can provide (a) a molded product with a low VOC generation amount (formaldehyde generation amount) and (b) good impact resistance by mixing the modifier with a polyacetal resin (C).

[0294] Industrial Applicability

[0295] The polyacetal resin composition using the polyacetal resin modifier of one embodiment of the present invention can be appropriately used for electrical and electronic applications, automotive parts applications, and industrial equipment applications. The polyacetal resin composition using the polyacetal resin modifier of one embodiment of the present invention can be appropriately used, for example, for driving mechanical parts of AV equipment, dishwashing and drying machine handles, speaker grilles, washing tank stirring propellers, OA equipment switches, gears, automotive wiper motor system gears, regulator handles, interior door handles, door lock side housings, gear shift levers, heater fans, pipe brackets, electric window regulators, seat belts, electric seat gears, sunroofs, clips, fasteners, industrial equipment conveyor screws, belt conveyors, chains, torque limiters, etc.

Claims

1. A modifier for polyacetal resin, The invention comprises a rubber-containing graft copolymer (A) and a polymer compound (B) having a glycidyl group, The rubber-containing graft copolymer (A) comprises an elastomer and a graft portion graft-bonded to the elastomer. The grafted portion is composed only of constituent units derived from a vinyl monomer having no reactive functional group, The mass ratio of the elastomer to the grafted portion, that is, the mass part of the elastomer / the mass part of the grafted portion, is 60 / 40 to 95 / 5, The content of chlorine in the polyacetal resin modifier is 1 ppm to 170 ppm based on the mass of the polyacetal resin modifier. The content of calcium in the polyacetal resin modifier is 1 ppm to 780 ppm based on the mass of the polyacetal resin modifier. The pH of a mixture consisting of 10 parts by mass of the polyacetal resin modifier and 100 parts by mass of deionized water is 6.0 to 8.

0.

2. The modifier for polyacetal resin according to claim 1, in, The polymer compound (B) is at least one of epoxidized soybean oil and epoxidized castor oil.

3. The modifier for polyacetal resin according to claim 1, in, The elastic body is composed only of (meth)acrylate rubber.

4. The modifier for polyacetal resin according to claim 1, in, The epoxy group content in the polyacetal resin modifier is 15 μmol / g to 180 μmol / g.

5. The modifier for polyacetal resin according to claim 1, in, The content of the polymer compound (B) in the polyacetal resin modifier is 0.1 to 5.0 parts by mass based on 100 parts by mass of the rubber-containing graft copolymer (A).

6. The modifier for polyacetal resin according to claim 1, in, The polyacetal resin modifier is in the form of powder or granules. 7 . A polyacetal resin composition comprising the polyacetal resin modifier according to claim 1 and a polyacetal resin (C).

8. The polyacetal resin composition according to claim 7, in, When the total of the polyacetal resin modifier and the polyacetal resin (C) is 100 mass %, the polyacetal resin modifier is 3 mass % to 80 mass %, and the polyacetal resin (C) is 20 mass % to 97 mass %. 9 . The polyacetal resin composition according to claim 7 , further comprising a formaldehyde scavenger.

10. The polyacetal resin composition according to claim 9, in, The formaldehyde scavenger comprises a reactive group reactive to formaldehyde. The content of the formaldehyde scavenger in the polyacetal resin composition is an amount in which the reactive group is 3.0 μmol or more based on 1 g of the total of the polyacetal resin modifier and the polyacetal resin (C).

11. The polyacetal resin composition according to claim 9, in, The formaldehyde scavenger includes one or more selected from the group consisting of hydrazide compounds, hydrazine compounds, guanamine compounds, and urea compounds.

12. A method for producing a modifier for polyacetal resin, include: a polymer compound (B) adding step of adding the polymer compound (B) having a glycidyl group in an emulsified state to the aqueous latex containing the rubber-containing graft copolymer (A); a coagulation step of adding calcium chloride to the aqueous latex obtained in the polymer compound (B) adding step to obtain a coagulation body comprising the rubber-containing graft copolymer (A) and the polymer compound (B); and a washing step of washing the agglomerates obtained in the agglomeration step; The rubber-containing graft copolymer (A) comprises an elastomer and a graft portion graft-bonded to the elastomer. The grafted portion is composed only of constituent units derived from a vinyl monomer having no reactive functional group, The mass ratio of the elastomer to the grafted portion, that is, the mass part of the elastomer / the mass part of the grafted portion, is 60 / 40 to 95 / 5, The pH of the aqueous latex is 5-9.