Preparation method of monatomic catalyst

By performing low-temperature segment drying and liquid-phase ultrasonic peeling in an inert atmosphere, the problems of high energy consumption and high production costs caused by high temperature treatment are solved, and the uniform distribution and good dispersion of single atomic catalyst are achieved, thereby reducing production cost and maintain the efficiency of the catalyst.

CN118949982AActive Publication Date: 2024-11-15NORTHWESTERN POLYTECHNICAL UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410949868.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-15
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing single-atom catalyst preparation method requires the treatment of foam transition metal in a high-temperature reduction atmosphere, resulting in large energy consumption and high production costs, which limits its practical application.

Method used

Using nitrogen-doped carbon material to heat treatment in an inert atmosphere, a graphene-like support material is obtained, and mixed with foam transition metal to dry in a protective atmosphere for low-temperature segmentation. Single-atom catalyst is formed by liquid phase ultrasonic peeling, eliminating high-temperature treatment step.

Benefits of technology

The uniform distribution and good dispersion of single-atom catalysts are achieved, the production cost is reduced, and the problem of high energy consumption caused by high temperature treatment is avoided. The effect of the prepared catalyst is comparable to that of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949982A_ABST
    Figure CN118949982A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a monatomic catalyst, which comprises the following steps: (1) carrying out heat treatment on a nitrogen-doped carbon material in an inert atmosphere to obtain a graphene-like carrier material; (2) mixing the graphene-like carrier material with a solvent, performing ultrasonic treatment to obtain graphene-like dispersion liquid, and performing low-temperature segmented drying in a protective atmosphere to obtain a foam metal-graphene-like material; (3) the foam metal-graphene-like material is subjected to liquid-phase ultrasonic stripping, and a monatomic catalyst is obtained; compared with the prior art, high-temperature treatment of the foam transition metal in a reducing atmosphere is omitted, and compared with a traditional high-temperature (500 DEG C or above) treatment method large in energy consumption, the method is milder and lower in production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanomaterials, and in particular relates to a method for preparing a single-atom catalyst. Background Art

[0002] With the development of nanocatalysis and the advancement of characterization technology, researchers have found that surface unsaturated coordinated atoms are often active sites of catalysis, so researchers control the size, morphology, and crystal plane of nanocrystals to regulate the distribution and structure of atoms on the catalyst surface to improve catalytic performance. When the size of nanocrystals is reduced to clusters and single atoms, their energy level structure and electronic structure will undergo fundamental changes. It is precisely because of this unique structural feature that single-atom catalysts often show activity, selectivity, and stability that are different from traditional nanocatalysts. Single-atom materials not only provide an ideal model and research platform for understanding the mechanism of catalytic reactions at the molecular level, but are also expected to become new catalysts with industrial catalytic applications and biomedical potential.

[0003] At present, the literature reports a variety of methods for preparing carbon-supported nitrogen-coordinated single-atom catalysts, such as impregnation pyrolysis, wet chemical synthesis, physical and chemical vapor deposition, electrochemical deposition, and ball milling.

[0004] In the invention patent with the public announcement number CN110801838A, a method for preparing a single-atom catalyst is disclosed, which is to subject the foamed transition metal to high-temperature treatment in a reducing atmosphere and then mix it with a graphene oxide dispersion. The high-temperature treatment temperature is 500°C to 900°C; the high-temperature treatment time is 1 to 3 hours.

[0005] In the above preparation method, the foamed transition metal needs to be treated at high temperature (above 500°C) in a reducing atmosphere. High temperature treatment consumes a lot of energy and has high production costs, which hinders the practical application of single-atom catalysts. Therefore, a preparation method with milder conditions is urgently needed to obtain single-atom catalysts with uniform atomic distribution. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing a single-atom catalyst, which eliminates the need for high-temperature treatment of the foamed transition metal in a reducing atmosphere. Compared with the traditional high-temperature (above 500°C) treatment method with high energy consumption, this method is milder and has lower production costs.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing a single atom catalyst comprises the following steps:

[0008] (1) heat treating the nitrogen-doped carbon material in an inert atmosphere to obtain a graphene-like carrier material;

[0009] (2) mixing a graphene-like carrier material with a solvent, ultrasonically preparing a graphene-like dispersion, mixing the prepared graphene-like dispersion with a foamed transition metal, and drying in a protective atmosphere to obtain a foamed metal-graphene-like material;

[0010] (3) subjecting the foamed metal-graphene-like material to liquid-phase ultrasonic exfoliation to obtain a single-atom catalyst;

[0011] In the step (2), the graphene-like dispersion obtained in the step (1) is evenly applied to a foam metal mesh with a mesh structure, and firstly treated at room temperature under an inert atmosphere for a period of time to remove surface ethanol and prevent oxidation of the foam metal; and then heated at a temperature below 100° C. under an inert atmosphere for a period of time to obtain a foam metal-graphene-like material.

[0012] Preferably, the solvent of the graphene-like carrier material in step (2) is ethanol.

[0013] Preferably, after the graphene-like dispersion and the foamed transition metal are mixed in step (2), drying is performed in a protective atmosphere in stages, first at room temperature for 10 to 12 hours, and then at 85 to 90° C. for 10 to 12 hours.

[0014] Preferably, the foam transition metal is one of cobalt, nickel and copper.

[0015] Preferably, the power of ultrasound during liquid phase ultrasonic stripping in step (3) is 800-1000W.

[0016] Preferably, the flow rate of the protective atmosphere gas during drying in step (2) is 50 mL / min to 80 mL / min.

[0017] Compared with the prior art, the present invention eliminates the need for high-temperature treatment of the foam transition metal in a reducing atmosphere, and adopts low-temperature segmented drying, first drying at room temperature for 10 to 12 hours, and then drying at 85 to 90°C for 10 to 12 hours. First, the foam copper is treated at room temperature for 12 hours, and ethanol is slowly removed to avoid oxidation of the foam copper. Then, after low-temperature treatment (85 to 90°C), the metal atoms on the surface of the foam metal are captured at low temperature (90°C) by using graphene-like surface dangling bonds in the process, and metal-oxygen coordination is formed to achieve the preparation of a single-atom catalyst. It can be seen from the characterization of spherical aberration-corrected transmission electron microscopy that the prepared single-atom catalyst metal single atoms are evenly distributed and have good dispersibility. Compared with the traditional high-temperature (above 500°C) treatment method with high energy consumption, this method is more gentle and has lower production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A schematic diagram of the synthesis of the single-atom catalyst provided by the present invention;

[0019] Figure 2 This is a spherical aberration corrected transmission electron microscopy image of a single copper atom in Example 1 of the present invention;

[0020] Figure 3 This is a spherical aberration corrected transmission electron microscopy image of a single cobalt atom in Example 2 of the present invention;

[0021] Figure 4 This is a spherical aberration corrected transmission electron microscopy image of a single nickel atom in Example 3 of the present invention. DETAILED DESCRIPTION

[0022] The following is a detailed description of the specific implementation methods in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation methods. The raw materials and reagents used in the examples are all commercially available unless otherwise specified.

[0023] like Figure 1 As shown, the present invention provides a method for preparing a single atom catalyst, comprising the following steps:

[0024] (1) heat treating the nitrogen-doped carbon material in an inert atmosphere to obtain a graphene-like carrier material;

[0025] (2) mixing a graphene-like carrier material with a solvent, ultrasonically preparing a graphene-like dispersion, mixing the prepared graphene-like dispersion with a foamed transition metal, and drying in a protective atmosphere to obtain a foamed metal-graphene-like material;

[0026] (3) subjecting the foamed metal-graphene-like material to liquid-phase ultrasonic exfoliation to obtain a single-atom catalyst;

[0027] The solvent of the graphene-like carrier material in step (2) is ethanol.

[0028] In the step (2), after the graphene-like dispersion is mixed with the foamed transition metal, it is dried in a protective atmosphere in a staged manner, first at room temperature for 10 to 12 hours, and then at 85 to 90° C. for 10 to 12 hours. In this process, the graphene-like surface dangling bonds are used to capture metal atoms on the surface of the foamed metal at a low temperature (90° C.) to form a metal-oxygen coordination.

[0029] The foam transition metal is one of cobalt, nickel and copper.

[0030] The foamed metal-graphene oxide material is subjected to liquid phase ultrasonic exfoliation to obtain a single atom catalyst, and the ultrasonic power during the liquid phase ultrasonic exfoliation in the step (3) is 800 to 1000W.

[0031] The flow rate of the protective atmosphere gas during the drying step (2) is 50 mL / min to 80 mL / min.

[0032] Example 1: Preparation of Cu single atom catalyst

[0033] (1) 2 g of melamine was heated at 600 °C in an argon atmosphere for 3 h to obtain a bulk carbon nitride material, and then heated at 500 °C in an argon atmosphere for 2 h to obtain about 100 mg of graphene-like powder.

[0034] (2) The above 20 mg of graphene-like material was mixed with 5 ml of ethanol and ultrasonicated (with a power of 800 W) for 30 min to obtain a graphene-like dispersion.

[0035] (3) The above dispersion was evenly dropped on a foam copper mesh (area 16 cm 2 , thickness 3mm), (the ratio of graphene-like dispersion to copper foam is 1ml:10g), dried under argon atmosphere with an argon flow rate of 50mL / min, treated at room temperature for 10h, and ethanol was slowly removed to avoid oxidation of copper foam.

[0036] (4) The above materials were placed in an argon atmosphere at a flow rate of 80 mL / min and treated at 90° C. for 10 h to obtain a foamed copper-graphene-like material.

[0037] (5) The foam copper-graphene-like material was dispersed in 100 mL of ethanol and subjected to ultrasound (power of 1000 W) for 3 h. The suspension was separated by centrifugation (2000 rpm, 10 min), washed with deionized water 3 times, washed with ethanol once, and vacuum dried at 40 ° C for 24 h to obtain a copper single atom catalyst.

[0038] (6) The copper single-atom catalyst obtained in Example 1 was characterized by spherical aberration-corrected transmission electron microscopy. The results are as follows: Figure 2 As shown by Figure 2 It can be seen that copper atoms are evenly dispersed on the graphene-like surface.

[0039] Example 2: Preparation of Co single atom catalyst

[0040] (1) 2 g of melamine was heated at 600 °C in an argon atmosphere for 3 h to obtain a bulk carbon nitride material, and then heated at 500 °C in an argon atmosphere for 2 h to obtain about 100 mg of graphene-like powder.

[0041] (2) The above 20 mg of graphene-like material was mixed with 5 ml of ethanol and ultrasonicated (with a power of 800 W) for 30 min to obtain a graphene-like dispersion.

[0042] (3) The above dispersion was evenly dropped onto a cobalt foam mesh (area 16 cm 2, thickness 3mm), (the ratio of graphene-like dispersion to cobalt foam is 1ml:10g), dried under argon atmosphere, the argon flow rate is 50mL / min, treated at room temperature for 11h, and ethanol is slowly removed to avoid oxidation of cobalt foam.

[0043] (4) The above materials were placed in an argon atmosphere at a flow rate of 80 mL / min and treated at 90° C. for 11 h to obtain a foamed cobalt-graphene-like material.

[0044] (5) The foamed cobalt-graphene-like material was dispersed in 100 mL of ethanol and subjected to ultrasound (power of 1000 W) for 3 h. The suspension was separated by centrifugation (2000 rpm, 10 min), washed with deionized water 3 times, washed with ethanol once, and vacuum dried at 40 ° C for 24 h to obtain a cobalt single atom catalyst.

[0045] (6) The cobalt single-atom catalyst obtained in Example 2 was characterized by spherical aberration-corrected transmission electron microscopy. The results are as follows: Figure 3 As shown by Figure 3 It can be seen that single cobalt atoms are evenly dispersed on the graphene-like surface.

[0046] Example 3: Preparation of Ni single atom catalyst

[0047] (1) 2 g of melamine was heated at 600 °C in an argon atmosphere for 3 h to obtain a bulk carbon nitride material, and then heated at 500 °C in an argon atmosphere for 2 h to obtain about 100 mg of graphene-like powder.

[0048] (2) The above 20 mg of graphene-like material was mixed with 5 ml of ethanol and ultrasonicated (with a power of 800 W) for 30 min to obtain a graphene-like dispersion.

[0049] (3) The above dispersion was evenly dropped onto a nickel foam mesh (area 16 cm 2 , thickness 3mm), (the ratio of graphene-like dispersion to nickel foam is 1ml:10g), dried under argon atmosphere, the argon flow rate is 50mL / min, treated at room temperature for 12h, and ethanol is slowly removed to avoid oxidation of nickel foam.

[0050] (4) The above materials were continued to be placed in an argon atmosphere with an argon flow rate of 80 mL / min and treated at 85° C. for 12 h to obtain a foamed nickel-graphene-like material.

[0051] (5) The foamed cobalt-graphene-like material was dispersed in 100 mL of ethanol and subjected to ultrasound (power of 1000 W) for 3 h. The suspension was separated by centrifugation (2000 rpm, 10 min), washed with deionized water 3 times, washed with ethanol once, and vacuum dried at 40 ° C for 24 h to obtain a nickel single atom catalyst.

[0052] (6) The nickel single-atom catalyst obtained in Example 3 was characterized by spherical aberration-corrected transmission electron microscopy. The results are as follows: Figure 4 As shown by Figure 4 It can be seen that nickel atoms are evenly dispersed on the graphene-like surface.

[0053] The innovation of the present invention is that it eliminates the need for high-temperature treatment of the foam transition metal in a reducing atmosphere, and adopts low-temperature segmented drying, first drying at room temperature for 10 to 12 hours, and then drying at 85 to 90° C. for 10 to 12 hours. First, it is treated at room temperature for 12 hours, and ethanol is slowly removed to avoid oxidation of the foam copper. Then, after low-temperature treatment (85 to 90° C.), in this process, the metal atoms on the surface of the foam metal are captured at low temperature (90° C.) by using the graphene-like surface dangling bonds, and metal-oxygen coordination is formed to achieve the preparation of the single-atom catalyst. It can be seen from the characterization of the spherical aberration-corrected transmission electron microscope that the prepared single-atom catalyst metal single atoms are evenly distributed and have good dispersibility. Compared with the traditional high-temperature (above 500° C.) treatment method with high energy consumption, the prepared catalyst has the same effect, but the method is milder and has a lower production cost.

Claims

1. A method for preparing a single-atom catalyst, characterized in that: The steps include: (1) heat-treating the nitrogen-doped carbon material in an inert atmosphere to obtain a graphene-like carrier material; (2) mixing a graphene-like carrier material with a solvent, ultrasonically preparing a graphene-like dispersion, mixing the prepared graphene-like dispersion with a foamed transition metal, and drying in a protective atmosphere to obtain a foamed metal-graphene-like material; (3) subjecting the foamed metal-graphene-like material to liquid-phase ultrasonic exfoliation to obtain a single-atom catalyst; In the step (2), the graphene-like dispersion obtained in the step (1) is evenly applied to a foam metal mesh having a mesh structure, and first placed in an inert atmosphere at room temperature for a period of time to remove surface ethanol and prevent oxidation of the foam metal; and then heated at below 100° C. in the inert atmosphere for a period of time to obtain a foam metal-graphene-like material.

2. The method for preparing a single-atom catalyst according to claim 1, wherein: The solvent of the graphene-like carrier material in step (2) is ethanol.

3. The method for preparing a single-atom catalyst according to claim 1, wherein: In the step (2), after the graphene-like dispersion is mixed with the foamed transition metal, drying is performed in a protective atmosphere in a stepwise manner, first at room temperature for 10 to 12 hours, and then at 85 to 90° C. for 10 to 12 hours.

4. The method for preparing a single-atom catalyst according to claim 1, wherein: The foam transition metal is one of cobalt, nickel and copper.

5. The method for preparing a single-atom catalyst according to claim 1, wherein: The ultrasonic power during the liquid phase ultrasonic stripping in step (3) is 800-1000W.

6. The method for preparing a single-atom catalyst according to claim 3, characterized in that: The flow rate of the protective atmosphere gas during the drying step (2) is 50 mL / min to 80 mL / min.

Citation Information

Patent Citations

  • Preparation method of foamed nickel carrying carbonitride / reduced graphene photocatalyst

    CN107020142A

  • Nitrogen carbide nanosheet and preparation method and application thereof

    CN107311125A

  • Preparation method of monatomic catalyst

    CN110801838A

  • Precious metal monatomic catalyst and preparation method thereof

    CN114618550A