Copper flat wire drawing process and device
By combining the special mold drawing method and the rolling method, a blank line with a moderate width and thickness ratio is first formed and roll extruded, the problem of the limited and low pass rate of copper flat line production in the prior art is solved, and a high The width and thickness are lower cost and high pass rate production than copper wire.
Patent Information
- Application Number
- CN202411204939.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In the existing copper flat wire production process, the special-shaped mold drawing method cannot produce copper flat wire with a width-thickness ratio of more than 2.5, and the strip longitudinal shearing method is difficult to produce copper flat wire with a width of less than 3mm, and the pass rate is low, so the rolling method is not suitable. The production of conventional copper flat wires leads to high costs and unqualified products.
Using a process combining special-shaped die drawing method and rolling method, the thick wire is first drawn into a blank line with a width-thickness ratio of less than 2, and a flying wing is formed on both sides of the blank line. The flying wing and the blank line are extruded by rollers. The side walls are joined to form a blank line with a high width and thickness ratio, and then a second pull is performed to ensure a high pass rate and low cost of the product.
The production of high-width and thickness ratio copper wire is achieved while reducing costs and improving product qualification rate, avoiding sickle bending and wire twisting, and ensuring the high quality and use effect of copper flat wire.
Smart Images

Figure CN118950728A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of copper flat wires, and in particular relates to a copper flat wire drawing process and a device. Background Art
[0002] Copper flat wire is the main material used to make enameled flat wire, and its production process includes special-shaped die drawing method, strip slitting method and rolling method.
[0003] The special-shaped die drawing method uses a special-shaped wire drawing die with a rectangular hole shape to draw a thick wire with a rectangular cross-section. It has low cost, but can only produce copper flat wires with a low aspect ratio. When used to produce copper flat wires with a aspect ratio exceeding 2.5, it is prone to breakage.
[0004] Strip slitting method uses a slitting unit to cut wide strips to obtain narrow strips with a minimum width of about 3mm. The advantages of the strip slitting process are that it is easy to process and can obtain copper flat wires with a large aspect ratio. The processing cost is low in the case of large width. However, the disadvantage is that the lateral tension during the cutting process is extremely easy to cause sickle bending and wire kinking, making the product unqualified.
[0005] The rolling method first draws the copper material to a precise wire diameter by a round wire drawing method, and then passes through multiple flat rollers to flatten and roll it into shape. The rolling method can produce copper flat wires with a large width-to-thickness ratio, but it requires more expensive equipment investment and more stringent production processes. It is generally only used in the production of ultra-thin copper flat wires (thickness less than 0.2mm). It is not suitable for conventional copper flat wires (thickness above 0.5mm) in terms of cost, and the resulting copper flat wires will have cracks on both sides due to rolling. Figure 6 The arc surface shown in the figure will reduce the slot fill rate when the enameled flat wire made of copper flat wire is used for winding, and the use effect is not very good.
[0006] Among the above three processes, the special die drawing method has the lowest cost, the strip slitting method has the second lowest cost, and the rolling method has the highest cost. The special die drawing method cannot be used to produce copper flat wires with a width-to-thickness ratio of more than 2.5; the strip slitting method cannot be used to produce copper flat wires with a width of less than 3mm, and the qualified rate is low; the rolling method is not suitable for the production of conventional copper flat wires. Summary of the invention
[0007] The object of the present invention is to provide a copper flat wire drawing process and device. The present invention can produce copper wires with high aspect ratio, low cost and high qualified rate.
[0008] The technical solution of the present invention is a copper flat wire drawing process, comprising the following steps:
[0009] a. Take a thick wire, and use a special-shaped die drawing method to obtain a blank wire according to the width and thickness of the copper flat wire to be obtained. The width-to-thickness ratio of the blank wire is less than 2, the thickness of the blank wire is 1.5-3 times the thickness of the copper flat wire, and wings are formed on both sides of the width of the blank wire. The cross-sectional area of the blank wire is 1.05-1.2 times the cross-sectional area of the copper flat wire, and the thickness of the wings is 1.05-1.1 times the thickness of the copper flat wire;
[0010] b. Rolling a blank wire with a power-driven pair of rollers, so that the thickness of the blank wire is squeezed toward both sides to be flush with the wing, thereby obtaining a second blank wire;
[0011] c. Use the special-shaped die drawing method to draw the two-pass billet wire into copper flat wire.
[0012] In the above-mentioned copper flat wire drawing process, the two side walls in the thickness direction of the blank wire are connected to the corresponding wings at an inclined surface, and a rounded corner is provided at the connection point.
[0013] The device for realizing the aforementioned copper flat wire drawing process includes a frame. Viewed from the moving direction of the copper flat wire, the frame is provided with a first shaped wire drawing die, a pair of rollers and a second shaped wire drawing die in sequence. The first shaped wire drawing die is provided with a drawing hole, the pair of rollers is connected with a driving mechanism, and the second shaped wire drawing die is provided with two drawing holes.
[0014] In the aforementioned device, the single-shaped wire drawing die and the double-shaped wire drawing die both include a template connected to a frame, the template is provided with a mounting hole, a module is provided at the mounting hole, the module is connected to the template with screws, and the module is provided with one or two drawing holes.
[0015] In the aforementioned device, both ends of the first wire drawing hole and both ends of the second wire drawing hole expand outwards to form bell mouths.
[0016] In the aforementioned device, an oil tank is provided at the bottom of the frame, an oil pump is provided in the oil tank, and oil injection pipes connected to the oil pump are provided on the front and rear sides of one drawing hole, the front and rear sides of the rollers, and the front and rear sides of the second drawing hole.
[0017] In the aforementioned device, valves are provided on each of the six fuel injection pipes.
[0018] In the aforementioned device, a cavity is formed between the frame, the first special-shaped wire drawing die and the second special-shaped wire drawing die, and the cavity is connected to a gas source of nitrogen or carbon dioxide through an air pipe, and an air valve is provided on the air pipe.
[0019] In the aforementioned device, the pair of rollers includes an active roller and a passive roller located above the active roller. Both ends of the active roller are rotatably connected to the frame. The frame is provided with a motor, which is connected to the active roller through a magnetic coupling. Both ends of the passive roller are provided with sliders connected to the frame, and fasteners are provided between the sliders and the frame.
[0020] In the aforementioned device, the output speed of the motor is greater than the rotation speed of the active roller, the maximum transmission torque of the magnetic coupling is converted by the active roller into the traction force of the two blank wires, and the sum of the resistance of one blank wire passing through the pair of rollers and the resistance of the thick wire passing through a special-shaped wire drawing die is greater than the traction force of the active roller on the two blank wires.
[0021] Compared with the prior art, the present invention combines the existing special-shaped die drawing method and rolling method, and first draws the thick wire rod for the first time. During the first drawing, the thick wire rod is first drawn into a blank wire, and the width-to-thickness ratio of the blank wire is less than 2, so as to ensure that the blank wire has good rigidity and will not be broken, and form wings with a thickness similar to that of the copper flat wire to be obtained on both sides of the blank wire. Although the wings are relatively thin, they will not crack due to the narrow width, so as to ensure smooth drawing. After the first drawing is completed, the wings are extruded by the rollers. During the extrusion, the wing parts are basically not deformed by the extrusion, so as to ensure that the outer wall of the wings will not bend to form a circular arc surface, so as to improve the use effect of the obtained copper flat wire. At the same time, the vertical force of the roller extrusion deforms the blank wire, which is different from the tensile force that deforms the blank wire, so that the blank wire will not break, and can be formed into two blank wires with a high flatness ratio. After the roller extrusion, the second drawing is performed. During the second drawing, since the second blank wire and the copper flat wire are similar in shape, the deformation margin is small, and the drawing resistance is small, ensuring that the second blank wire is not easy to break. Since there is no lateral tension during drawing and roller extrusion, the obtained copper flat wire will not produce sickle bending and wire material twisting, and the product qualification rate is high. Therefore, the present invention can produce the advantages of high aspect ratio copper wire, and the cost is low and the qualification rate is high.
[0022] In the device, when producing copper flat wires of different specifications, it is only necessary to replace the corresponding modules and adjust the clearance of the rollers, which has a wide range of applications. At the same time, spraying wire drawing oil not only further reduces the possibility of copper wire breakage, but also protects the copper wire from oxidation and avoids the reduction of copper wire quality. The motor drives the rollers to rotate through the magnetic coupling to ensure that the motor speed does not affect the moving speed of the copper wire, and ensure that the driving force of each position of the copper wire is reasonably distributed. The copper wire always moves in a taut state to avoid the formation of knotted areas, ensuring the smooth progress of production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the front view of the device.
[0024] Figure 2 This is a left view schematic diagram of a special-shaped wire drawing die.
[0025] Figure 3 It is a left view schematic diagram of a two-pass special-shaped wire drawing die.
[0026] Figure 4 It is a left view schematic diagram of the rollers.
[0027] Figure 5 This is a schematic cross-sectional view of a blank wire.
[0028] Figure 6 It is a schematic cross-sectional view of a copper flat wire obtained by an existing rolling method.
[0029] The marks in the accompanying drawings are: 1-copper flat wire, 2-a blank wire, 3-wings, 4-two blank wires, 5-rounded corners, 6-frame, 7-a special-shaped wire drawing die, 8-pair of rollers, 9-two special-shaped wire drawing dies, 10-a drawing hole, 11-two drawing holes, 12-template, 13-mounting hole, 14-module, 15-bell mouth, 16-oil tank, 17-oil pump, 18-injection pipe, 19-valve, 20-cavity, 21-air pipe, 22-air valve, 23-active roller, 24-passive roller, 25-slider, 26-fastener, 27-motor, 28-magnetic coupling, 29-notch. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0031] Embodiment 1. A copper flat wire drawing process comprises the following steps: a. A thick wire with a rectangular cross section is taken, and according to the width and thickness of the copper flat wire 1 to be obtained, the copper flat wire 1 is taken as an example of 5 mm in width and 1 mm in thickness in Embodiment 1, and a blank wire 2 is obtained by a special-shaped die drawing method, wherein the width-to-thickness ratio of the blank wire 2 is less than 2, and the thickness of the blank wire 2 is 1.5-3 times the thickness of the copper flat wire 1. In Embodiment 1, the thickness is T1=1.8 mm, and wings 3 are formed on both sides of the blank wire 2 in the width direction, and two side walls of the blank wire 2 in the thickness direction are connected to the corresponding wings 3 at an inclined surface, and a fillet 5 for transition is provided at the connection. The cross-sectional area of a blank wire 2 is 1.05-1.2 times the cross-sectional area of the copper flat wire 1, the thickness T2 of the wing 3 is 1.05-1.1 times the thickness of the copper flat wire 1, and the thickness T2=1.05mm in Example 1. The width L1 of the wing 3 is 0.1-0.2 times the width of the copper flat wire 1, and L1 is 1mm in Example 1. The wing 3 is not subjected to extrusion during the subsequent rolling process.
[0032] b. Rolling a blank wire 2 by using a pair of power-driven rollers 8, so that the thickness of the blank wire 2 is squeezed toward both sides to be flush with the wing 3, thereby obtaining a second blank wire 4, wherein the thickness of the second blank wire 4 is 1.05 mm and the width is 5.05 mm;
[0033] c. The second blank wire 4 is drawn into a copper flat wire 1 by a special-shaped die drawing method.
[0034] Embodiment 2. The device for implementing the process of embodiment 1 comprises a frame 6. When viewed from the moving direction of the copper flat wire 1, the frame 6 is provided with a single-shaped wire drawing die 7, a pair of rollers 8 and a second-shaped wire drawing die 9 in sequence. The single-shaped wire drawing die 7 is provided with a wire drawing hole 10, and the shape of the single-shaped wire drawing hole 10 matches the shape of the single-blade wire 2. The pair of rollers 8 is connected with a driving mechanism. The second-shaped wire drawing die 9 is provided with two wire drawing holes 11, and the shape of the two wire drawing holes 11 matches the shape of the second-blade wire 4.
[0035] The single-shaped wire drawing die 7 and the second-shaped wire drawing die 9 both include a template 12 connected to the frame 6, the template 12 is provided with a mounting hole 13, the mounting hole 13 is provided with a module 14, the module 14 is screwed to the template 12, and the module 14 is provided with a single drawing hole 10 or two drawing holes 11.
[0036] Both ends of the first wire drawing hole 10 and both ends of the second wire drawing hole 11 expand outwards to form bell mouths 15 .
[0037] An oil groove 16 is provided at the bottom of the frame 6, and the first wire drawing hole 10, the pair of rollers 8 and the second wire drawing hole 11 are all located above the oil groove 16. An oil pump 17 is provided in the oil groove 16, and the front and rear sides of the first wire drawing hole 10, the front and rear sides of the pair of rollers 8 and the front and rear sides of the second wire drawing hole 11 are all provided with an oil injection pipe 18 connected to the oil pump 17, and the oil injection pipe 18 can be fixed to the frame 6 through a connecting piece.
[0038] The six fuel injection pipes 18 are all provided with valves 19 .
[0039] A cavity 20 is formed between the frame 6, the first special-shaped wire drawing die 7 and the second special-shaped wire drawing die 9. The cavity 20 is connected to a gas source of nitrogen or carbon dioxide through an air pipe 21. The outlet of the gas source is provided with a pressure reducing valve to achieve low-pressure gas discharge. An air valve 22 is provided on the air pipe 21. A notch 29 is provided at the bottom of the template 12. The liquid level of the drawing oil in the oil tank 16 exceeds the notch 29, which prevents nitrogen or carbon dioxide from leaking out of the cavity 20 and leaves a passage for the corresponding oil injection pipe 18 to extend out of the cavity 20.
[0040] The pair of rollers 8 includes an active roller 23 and a passive roller 24 located above the active roller 23. Both ends of the active roller 23 are rotatably connected to the frame 6. The frame 6 is provided with a motor 27. The motor 27 is connected to the active roller 23 through a magnetic coupling 28. Both ends of the passive roller 24 are provided with sliders 25 connected to the frame 6. A fastener 26 is provided between the slider 25 and the frame 6. The slider 25 is provided with a vertical long hole. The fastener 26 is a bolt that passes through the long hole and is connected to the frame 6. When the bolt is loosened, the slider 25 can move up and down to change the height of the passive roller 24 and the gap between the pair of rollers. It is suitable for the production of copper flat wires of different thicknesses.
[0041] The output speed of the motor 27 is greater than the rotation speed of the active roller 23, and the maximum transmission torque of the magnetic coupling 28 is converted by the active roller 23 into the traction force of the second blank wire 4. The sum of the resistance of the first blank wire 2 passing through the counter roller 8 and the resistance of the thick wire passing through the first special-shaped wire drawing die 7 is greater than the traction force of the active roller 23 on the second blank wire 4. In other words, it is impossible to make the copper wire pass through the first special-shaped wire drawing die 7 and the counter roller 8 by relying solely on the counter roller. It is necessary to obtain a small part of the traction force on the copper flat wire 1. The traction force on the copper flat wire 1 comes from the drawing machine, which ensures that the second blank wire 4 will not be piled up between the counter roller and the second special-shaped wire drawing die 9, ensuring the smooth progress of production. This can be achieved by selecting an appropriate magnetic coupling 28, and the traction force of the counter roller 8 is limited by the magnetic coupling 28.
[0042] The method of using Example 2: The device is fixed on the drawing machine, and the thick wire is wound on the feeding mechanism of the drawing machine. The thick wire passes through a drawing hole 10, a pair of rollers 8, and two drawing holes 11 to become a copper flat wire 1, which is then connected to the receiving mechanism of the drawing machine. The receiving mechanism winds the copper flat wire 1 and gives traction to the copper flat wire 1.
[0043] The oil pump 17 pumps the stretching oil in the oil tank 16, and the stretching oil is sprayed out from the oil spray pipe 18. By adjusting the opening of each valve 19, the amount of oil sprayed from each oil spray pipe 18 is similar or the same. The oil spray pipe 18 located in front of the first wire drawing hole 10, the roller 8, and the second wire drawing hole 11 mainly plays a lubricating role, reduces the stretching resistance, and avoids the copper wire from breaking. At the same time, it reduces the wear of the module 14 and reduces the maintenance frequency. The oil spray pipe 18 located on the back side of the first wire drawing hole 10, the roller 8, and the second wire drawing hole 11 mainly plays a role in cooling the copper wire to avoid oxidation of the copper wire and reduce its quality. At the same time, the low-temperature mechanical properties of the copper wire will not decrease, and to a certain extent, it can also prevent the copper wire from breaking.
[0044] The nitrogen or carbon dioxide in the gas source is introduced into the cavity 20 through the gas pipe to reduce the oxygen content in the cavity 20, further avoid oxidation of the copper wire, and improve the quality of the copper flat wire 1. The stretching oil in the oil tank 16 is first removed, and nitrogen or carbon dioxide is introduced at a large flow rate, and then the stretching oil is returned to the oil tank 16, so that the outside air cannot enter the cavity 20. At this time, the gas valve 22 is kept at a small opening, and nitrogen or carbon dioxide is slowly added to the cavity 20, thereby reducing the gas consumption and reducing the production cost.
Claims
1. A copper flat wire drawing process, characterized by: Includes the following steps, a. Take a thick wire and, according to the width and thickness of the copper flat wire (1) to be obtained, use the special die drawing method to obtain a blank wire (2). The width-to-thickness ratio of the blank wire (2) is less than 2. The thickness of the blank wire (2) is 1.5-3 times the thickness of the copper flat wire (1). The width of the blank wire (2) forms wings (3) on both sides. The cross-sectional area of the blank wire (2) is 1.05-1.2 times the cross-sectional area of the copper flat wire (1). The thickness of the wings (3) is 1.05-1.1 times the thickness of the copper flat wire (1). b. Use the power-driven rollers (8) to roll a first blank line (2), so that the thickness of the first blank line (2) is squeezed to both sides until it is flush with the flying wing (3) to obtain a second blank line (4). c. The two blanks (4) are drawn into copper flat wires (1) using the special die drawing method.
2. The copper flat wire drawing process according to claim 1, characterized in that: The two sidewalls of the first blank line (2) in the thickness direction are connected to the inclined surface between the corresponding flying wing (3), and a rounded corner (5) is provided at the connection point.
3. An apparatus for implementing the copper flat wire drawing process as described in claim 1 or 2, characterized in that: The frame (6) includes a first shaped wire drawing die (7), a pair of rollers (8) and a second shaped wire drawing die (9) arranged sequentially on the frame (6) from the direction of movement of the copper flat wire (1). The first shaped wire drawing die (7) has a wire drawing hole (10), the pair of rollers (8) is connected to a drive mechanism, and the second shaped wire drawing die (9) has two wire drawing holes (11).
4. The apparatus according to claim 3, characterized in that: Both the first-stage irregular wire drawing die (7) and the second-stage irregular wire drawing die (9) include a template (12) for connecting the frame (6). The template (12) is provided with mounting holes (13), and a module (14) is provided at the mounting holes (13). The module (14) is screwed to the template (12), and the module (14) is provided with one wire drawing hole (10) or two wire drawing holes (11).
5. The apparatus according to claim 4, characterized in that: Both ends of the first wire drawing hole (10) and both ends of the second wire drawing hole (11) expand outward to form a trumpet mouth (15).
6. The apparatus according to claim 3, characterized in that: The bottom of the frame (6) is provided with an oil tank (16), and an oil pump (17) is provided in the oil tank (16). The front and rear sides of the first wire drawing hole (10), the front and rear sides of the roller (8) and the front and rear sides of the second wire drawing hole (11) are all provided with oil spray pipes (18) connected to the oil pump (17).
7. The apparatus according to claim 6, characterized in that: Each of the six fuel injection pipes (18) is equipped with a valve (19).
8. The apparatus according to claim 6, characterized in that: The frame (6), the first shaped wire drawing die (7) and the second shaped wire drawing die (9) form a cavity (20). The cavity (20) is connected to a nitrogen or carbon dioxide gas source through a gas pipe (21). A gas valve (22) is provided on the gas pipe (21).
9. The apparatus according to claim 3, characterized in that: The rollers (8) include a drive roller (23) and a passive roller (24) located above the drive roller (23). Both ends of the drive roller (23) are rotatably connected to the frame (6). The frame (6) is equipped with a motor (27), which is connected to the drive roller (23) through a magnetic coupling (28). Both ends of the passive roller (24) are equipped with sliders (25) that connect to the frame (6). Fasteners (26) are provided between the sliders (25) and the frame (6).
10. The apparatus according to claim 9, characterized in that: The output speed of the motor (27) is greater than the rotation speed of the drive roller (23). The maximum transmission torque of the magnetic coupling (28) is converted into the traction force of the two blanks (4). The sum of the resistance of the first blank (2) when it passes through the roller (8) and the resistance of the thick wire when it passes through the shaped drawing die (7) is greater than the traction force of the drive roller (23) on the second blank (4).
Citation Information
Patent Citations
Equipment for producing small-sized copper flat wire
CN101486146A
Full automatic processing process for profiled enamel wire and system thereof
CN105070411A
Preparation method of ultrathin copper busbar for electricians
CN111653397A
Ultra-width-to-thickness-ratio copper bar preparation process and application thereof in copper bar production
CN117282794A
Enameled flat wire drawing die
CN210125650U
Cited By
Enameled copper wire drawing equipment
CN119346640A