Mass spectrometer interface cone preparation method

Through the double-sided welding technology of high-purity high-temperature resistant materials and high-thermal conductivity materials, combined with special structural design and high-precision welding technology, the problem of poor durability of ICP-MS interface cones in high-temperature and strong acid-base environments is solved, and long-term work and Low cost production.

CN118951616APending Publication Date: 2024-11-15GRIKIN ADVANCED MATERIALS
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411250032.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing ICP-MS interface cones have poor durability in high temperature and strong acid-base environments, short service life, and traditional processes are difficult to achieve multi-material composite structure design, resulting in waste of materials and high production costs.

Method used

The double-sided welding technology of high-purity high-temperature resistant materials and high-thermal conductivity materials is adopted to increase the contact area and thermal conductivity through special structural design, and combine electron beam or laser welding technology to improve the hardness and thermal conductivity of the cone material.

Benefits of technology

It realizes long-term working capacity under high-temperature corrosion conditions, reduces material waste and production costs, and improves detection sensitivity and low background interference performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951616A_ABST
    Figure CN118951616A_ABST
Patent Text Reader

Abstract

The invention discloses a mass spectrometer interface cone preparation method. Comprising the steps that corresponding contact surfaces and upper and lower welding parts are machined on the periphery of a flange of a conical opening blank part and the inner periphery of a round hole of a base plate blank part to obtain a conical opening part and a base plate part; and the contact surfaces of the conical opening component and the substrate component are bonded, and double-sided welding is carried out on the upper and lower welding parts. The high-melting-point conical opening material is selected, the hardness of the conical opening material is improved by adopting a hardening treatment process, and the high-temperature resistance, the high heat-conducting property and the use durability are ensured by combining the composite use of the high-heat-conducting substrate material. The design of a composite high-precision matching structure of different materials and a special contact surface structure is adopted, the use amount of expensive conical opening materials is reasonably set while the excellent performance of different materials is utilized, and the requirement for long-time work under the severe high-temperature corrosion condition is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inductively coupled plasma mass spectrometry (ICP-MS), and specifically relates to a method for preparing an inductively coupled plasma mass spectrometry sampling cone welding structure used for ICP-MS. Background Art

[0002] Inductively coupled plasma mass spectrometry (ICP-MS) technology is an inorganic element and isotope analysis and testing technology developed in the 1980s. It is a highly sensitive analysis technology that combines the high-temperature ionization characteristics of inductively coupled plasma with the advantages of sensitive and fast scanning of mass spectrometer through a unique interface device. ICP-MS mainly consists of three parts: ICP source, interface device and mass spectrometry analysis module. The interface cone component is the main component of the interface device, usually composed of a sampling cone and a skimmer cone. The interface cone component plays a key role in the transmission efficiency of the ion flow, has a great influence on the sensitivity, and directly determines the detection limit and stability of the instrument. The working environment of the interface cone component is harsh, and it is in a high temperature (above 1000°C) and acid-base environment. Therefore, the interface cone component is required to meet the requirements of high temperature resistance, corrosion resistance and good thermal conductivity.

[0003] Patent US5793039A discloses a mass spectrometer, a skimmer cone assembly, a skimmer cone and a manufacturing method thereof, wherein the cone is molded, and the manufacturing method thereof is significantly easier than mechanical processing, thereby reducing production costs.

[0004] Patent WO2018163576A1 discloses a plasma cone for an inductively coupled plasma mass spectrometer, an inductively coupled plasma mass spectrometer, and a method for manufacturing a plasma cone for an inductively coupled plasma mass spectrometer. Platinum, platinum group metals other than platinum, alloys, or alloy films thereof are plated on the surface of the plasma cone by various coating methods. The invention can reduce the impurity background without sacrificing sensitivity (ionic strength) and further improve the durability of the cone.

[0005] Patent CN2510862Y discloses an inductively coupled plasma mass spectrometry interface device, which consists of a sampling cone and a skimmer cone. The sampling cone and the skimmer cone are axially concentric. The sampling cone and the skimmer cone have a cone hole end thickness of 0.2 mm to 0.5 mm and are made of corrosion-resistant and high-temperature resistant metal materials.

[0006] The interface cones in existing patents have a single product structure and material or a small bonding area of ​​different materials, insufficient bonding, poor high temperature resistance, and are therefore easy to deform and have a short service life. In addition, there are few existing patents involving the preparation process of mass spectrometer interface cones. In order to meet special detection requirements such as strong corrosive acids, high matrix, and low detection limits, it is necessary to use precious metal materials with more stable chemical properties. Traditional compression molding or mechanical processing processes are difficult to design multi-material composite structures, and it is difficult to achieve long-term use of interface cones in high temperature and strong acid and alkali corrosion working environments. The large-scale use of precious metal materials not only increases production costs and causes material waste, but also fails to achieve long-term use of interface cones. Summary of the invention

[0007] In view of the problems existing in the background technology, the present invention provides a method for preparing a mass spectrometer interface cone, and the technical solution is as follows:

[0008] The corresponding contact surfaces and upper and lower welding parts are processed on the outer periphery of the flange of the tapered blank component and the inner periphery of the circular hole of the substrate blank component to obtain the tapered component and the substrate component;

[0009] The contact surfaces of the tapered part and the base part are fitted together, and double-sided welding is performed on the upper and lower welding parts.

[0010] The matching clearance of the contact surfaces is ≤0.05mm.

[0011] The contact surface is a special structural design for increasing the contact area, and the special structural design includes: cutting teeth, bevels, grooves or bumps.

[0012] The cone mouth blank component is made of a cone mouth material with a melting point greater than 1200°C.

[0013] The hardness of the cone mouth material is ≥80HV.

[0014] The cone mouth material is a high-purity material that is resistant to high temperatures and corrosion, and the content of impurity elements is ≤100ppm.

[0015] The cone mouth material includes: high-purity nickel, high-purity platinum and platinum alloy.

[0016] The substrate blank component is made of a high thermal conductivity material with a thermal conductivity greater than 90 W / (m·K).

[0017] The mass spectrometer interface cone blank component obtained after double-sided welding is subjected to precision machining and surface polishing.

[0018] The welding techniques used for the double-sided welding include: electron beam welding and laser welding.

[0019] The beneficial effects of the present invention are:

[0020] 1. Select cone mouth materials with high melting point, improve the hardness of cone mouth materials through hardening treatment process, and combine with high thermal conductivity substrate (base) materials to ensure high temperature resistance, high thermal conductivity and durability.

[0021] 2. The cone mouth material is made of high-purity material to ensure the detection sensitivity and low background interference performance of the interface cone product.

[0022] 3. Use double-sided precision welding technology of heterogeneous materials, with small heat input, small heat-affected zone, small deformation, high welding bonding rate and good thermal conductivity; at the same time, adopt different materials composite high-precision matching structure and special contact surface structure design to utilize the excellent performance of different materials while reasonably setting the amount of expensive cone-mouth material. The preparation process is simple and the production cost is low, which can meet the requirements of long-term work under severe high-temperature corrosion conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a process flow chart of a broad embodiment of a method for preparing a mass spectrometer interface cone of the present invention;

[0024] Figure 2 Schematic diagram of the mass spectrometer interface cone structure prepared in Examples 1 and 2 of the present invention;

[0025] Figure 3 It is a schematic diagram of the morphology of the fusion zone of the mass spectrometer interface cone welding provided in Examples 1 and 2 of the present invention;

[0026] Figure 4 Schematic diagram of the mass spectrometer interface cone structure prepared in Comparative Example 1 of the present invention;

[0027] Figure 5 Schematic diagram of the mass spectrometer interface cone structure prepared in Example 3 of the present invention;

[0028] Figure 6 Schematic diagram of the mass spectrometer interface cone structure prepared in Example 4 of the present invention;

[0029] Figure 7 It is a schematic diagram of the structure of the mass spectrometer interface cone prepared in Comparative Example 2 of the present invention.

[0030] Among them, 100 is a cone mouth component, 110 is a cone part, 111 is a tip cone surface, 112 is a large-angle cone surface, 113 is a cylinder, 120 is a flange part, 200 is a substrate component, 210 is a substrate body, and 220 is a mounting part. DETAILED DESCRIPTION

[0031] The present invention will be further described in detail below in conjunction with the accompanying drawings. The embodiments shown below are intended to make the advantages and features of the present invention more clear. They do not limit the invention contents described in the claims. In addition, the entire contents of the structures represented by the following embodiments are not limited to those necessary for the solutions of the invention described in the claims.

[0032] like Figure 1 The broad embodiment of the present invention shown comprises the following steps:

[0033] Step 1: Provide a cone-shaped block material with a melting point of more than 1200°C and a high thermal conductivity material circular plate with a thermal conductivity of more than 90W / (m·K);

[0034] Step 2: Processing the tapered block material into a tapered structure with a connecting flange as a tapered blank component, and processing a penetrating circular hole in the center of a high thermal conductivity material circular plate as a base plate blank component;

[0035] Step 3: Processing corresponding contact surfaces and upper and lower welding parts on the outer periphery of the flange of the tapered blank component and the inner periphery of the circular hole of the base plate blank component to obtain the tapered component and the base plate component, wherein the contact surface is a special structural design for increasing the contact area;

[0036] Step 4: Fit the contact surfaces of the cone mouth component and the base plate component, and then perform double-sided welding on the upper and lower welding parts to obtain the mass spectrometer interface cone blank component;

[0037] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0038] Specifically, the cone-mouth component 100 includes an integrated cone portion 110 and a flange portion 120. The cone inner end surface of the cone portion 110 includes at least one pointed cone surface 111. On the side of the pointed cone surface 111 facing the flange portion, at least one large-angle cone surface 112 or cylindrical surface 113 is provided as an extended inner surface as needed, extending all the way to the edge of the flange portion 120.

[0039] Specifically, the substrate body 210 of the substrate component 200 is in the shape of a circular plate. According to the position where the substrate component 200 needs to be installed, the large outer circle of the high thermal conductivity material circular plate is processed to form a mounting portion 220 in step 2; when used for a sampling cone, the mounting portion 220 is installed on the base of the water cooling disk through a clamping ring; when used for an intercepting cone, a thread is provided on the mounting portion 220 so as to be threadedly connected to the intercepting cone base.

[0040] Specifically, the cone block material is a high-purity material, including high-purity nickel, high-purity platinum, platinum alloy and other high-temperature and corrosion-resistant materials, and the impurity element content is ≤100ppm. By selecting high-purity materials as the materials of the cone parts, the detection sensitivity and low background interference performance of the interface cone products are guaranteed.

[0041] Specifically, the hardness of the cone mouth block material is ≥80HV; further, the high-purity cone mouth block material is hardened by work hardening, fine grain strengthening, etc. The high melting point cone mouth material is selected as the material of the cone mouth component, and the hardness of the cone mouth material is improved by using a hardening treatment process, combined with the composite use of a high thermal conductivity base material to ensure high temperature resistance, high thermal conductivity and durability;

[0042] Specifically, the high thermal conductivity material circular plate includes copper, copper alloy, etc.;

[0043] Specifically, the processing technology of the tapered block material includes spinning, stamping and other processes, and the tapered angle of the tapered structure is 30 to 150 degrees.

[0044] Specifically, the maximum diameter of the outer circumference of the flange of the tapered blank component is φ10-30 mm, and the minimum diameter of the through-type circular hole in the substrate blank component is also φ10-30 mm; the large outer diameter of the substrate blank component is 75-80 mm.

[0045] Specifically, the corresponding contact surfaces are all high-precision matching structures with a matching clearance of ≤0.05mm; the contact surfaces are specially designed in structure, and the special structural design enhances the cooling effect on the tapered material by increasing the contact area, and the special structural design includes: cutting teeth, bevels, grooves, bumps or a combination thereof.

[0046] Specifically, the welding technologies used for double-sided welding include electron beam welding, laser welding, etc. The double-sided precision welding technology of heterogeneous materials has small heat input, small heat-affected zone, small deformation, high welding bonding rate and good thermal conductivity.

[0047] Specifically, the welding depth of the upper and lower welding parts is 3 to 5 mm, and the weld width is ≤ 2 mm.

[0048] Embodiment 1:

[0049] Step 1: Provide a cone material with a melting point of >1200℃ and a high thermal conductivity material with a thermal conductivity of >90W / (m·K);

[0050] Step 2: Process the cone-shaped block material into a cone-shaped structure, and process a through circular hole in the center of the high thermal conductivity material circular plate;

[0051] Step 3: The contact surface between the cone-mouth blank component and the base blank component is processed into a high-precision matching structure, and the upper and lower welding parts are processed at the same time;

[0052] Step 4: After the contact surfaces are fitted, double-sided welding is performed on the upper and lower welding parts;

[0053] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0054] Specifically, the cone mouth material described in step 1 is a platinum alloy, and the impurity element content is less than 100ppm.

[0055] Specifically, the platinum alloy material described in step 1 is hardened by work hardening, grain refinement, etc., and has a hardness of 90 HV.

[0056] Specifically, the high thermal conductivity material described in step 1 is high purity copper.

[0057] Specifically, the platinum alloy material forming process described in step 2 is sample stamping forming, and the cone angle of the conical structure is 120°.

[0058] Specifically, the diameters of the platinum alloy material parts at the welding positions described in step 2 are φ10mm and φ8mm respectively, the diameters of the through-type circular holes of the high-purity copper parts at the welding positions are φ10mm and φ8mm respectively, and the large outer diameter is 76mm.

[0059] Specifically, the contact surface clearance between the tapered material and the high thermal conductivity material described in step three is ≤0.05mm, the upper and lower surfaces are welded, and the two ends of the contact surface are sealed. The contact surface is a structural design combining a bevel and a toothed surface. The bevel angle is 45°, the tooth tip angle is 60°, the tooth spacing is 0.4mm, and the tooth height is 0.4mm.

[0060] Specifically, step four adopts high energy electron beam welding.

[0061] Specifically, the welding depth of the component welding position described in step 4 is 3 mm, the welding width is 1.5 mm, and the welding bonding rate is 99%.

[0062] The interface cone structure prepared by the method of the present invention is as follows: Figure 2 As shown, when the metal solution signal drops to 1 / 4 at a high temperature plasma temperature of 1000°C in an inductively coupled plasma mass spectrometer, the usage time is >1200 hours.

[0063] Embodiment 2:

[0064] Step 1: Provide a cone material with a melting point of >1200℃ and a high thermal conductivity material with a thermal conductivity of >90W / (m·K);

[0065] Step 2: Process the cone-shaped block material into a cone-shaped structure, and process a through circular hole in the center of the high thermal conductivity material circular plate;

[0066] Step 3: The contact surface between the cone-mouth blank component and the base blank component is processed into a high-precision matching structure, and the upper and lower welding parts are processed at the same time;

[0067] Step 4: After the contact surfaces are fitted, double-sided welding is performed on the upper and lower welding parts;

[0068] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0069] Specifically, the cone mouth material described in step 1 is high-purity nickel, and the content of impurity elements is less than 100ppm.

[0070] Specifically, the high-purity nickel material described in step 1 is hardened by work hardening, grain refinement, etc., and its hardness is greater than 150 HV.

[0071] Specifically, the high thermal conductivity material described in step 1 is high purity copper.

[0072] Specifically, the high-purity nickel material forming process described in step 2 is sampled by stamping forming, and the cone mouth angle of the conical structure is 120°.

[0073] Specifically, the diameters of the high-purity nickel material parts at the welding positions described in step 2 are φ26mm and φ22mm respectively, the diameters of the through-type circular holes of the high-purity copper parts at the welding positions are φ26mm and φ22mm respectively, and the large outer diameter is 76mm.

[0074] Specifically, the contact surface size matching clearance between the high-purity nickel material component and the high thermal conductivity copper component described in step three is ≤0.05mm, the upper and lower surfaces are welded, and the two ends of the contact surface are sealed. The contact surface is a structural design combining a bevel and a toothed surface. The bevel angle is 45°, the tooth tip angle is 60°, the tooth spacing is 0.4mm, and the tooth height is 0.4mm.

[0075] Specifically, step four adopts high energy electron beam welding.

[0076] Specifically, the welding depth of the component welding position described in step 4 is 3 mm, the welding width is 1.5 mm, and the welding bonding rate is 99%.

[0077] The interface cone structure prepared by the method of the present invention is as follows: Figure 2 As shown, when the metal solution signal drops to 1 / 4 at a high temperature plasma temperature of 1000°C in an inductively coupled plasma mass spectrometer, the usage time is >1000 hours.

[0078] Embodiment 3:

[0079] Step 2: Process the cone-shaped block material into a cone-shaped structure, and process a through circular hole in the center of the high thermal conductivity material circular plate;

[0080] Step 3: The contact surface between the cone-mouth blank component and the base blank component is processed into a high-precision matching structure, and the upper and lower welding parts are processed at the same time;

[0081] Step 4: After the contact surfaces are fitted, double-sided welding is performed on the upper and lower welding parts;

[0082] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0083] Specifically, the cone mouth material described in step 1 is high-purity nickel, and the content of impurity elements is less than 100ppm.

[0084] Specifically, the high-purity nickel material described in step 1 is hardened by work hardening, grain refinement, etc., and its hardness is greater than 150 HV.

[0085] Specifically, the high thermal conductivity material described in step 1 is high purity copper.

[0086] Specifically, the high-purity nickel material forming process described in step 2 is sampled by stamping forming, and the cone mouth angle of the conical structure is 120°.

[0087] Specifically, the diameters of the high-purity nickel material parts at the welding positions described in step 2 are φ26mm and φ20mm respectively, the diameters of the through-type circular holes of the high-purity copper parts at the welding positions are φ26mm and φ20mm respectively, and the large outer diameter is 76mm.

[0088] Specifically, the contact surface size matching clearance between the high-purity nickel component and the copper component in step three is ≤0.05mm, the upper and lower surfaces are welded, the two ends of the contact surface are sealed, and the contact surface is designed with a bump structure with a width of 2mm and a height of 3mm.

[0089] Specifically, step four adopts high energy electron beam welding.

[0090] Specifically, the welding depth of the component welding position described in step 4 is 3 mm, the welding width is 1.5 mm, and the welding bonding rate is 99%.

[0091] The interface cone structure prepared by the method of the present invention is as follows: Figure 5 As shown, when the metal solution signal drops to 1 / 4 at a high temperature plasma temperature of 1000°C in an inductively coupled plasma mass spectrometer, the usage time is >1000 hours.

[0092] Embodiment 4:

[0093] Step 1: Provide a cone material with a melting point of >1200℃ and a high thermal conductivity material with a thermal conductivity of >90W / (m·K);

[0094] Step 2: Process the cone-shaped block material into a cone-shaped structure, and process a through circular hole in the center of the high thermal conductivity material circular plate;

[0095] Step 3: The contact surface between the cone-mouth blank component and the base blank component is processed into a high-precision matching structure, and the upper and lower welding parts are processed at the same time;

[0096] Step 4: After the contact surfaces are fitted, double-sided welding is performed on the upper and lower welding parts;

[0097] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0098] Specifically, the cone mouth material described in step 1 is high-purity nickel, and the content of impurity elements is less than 100ppm.

[0099] Specifically, the high-purity nickel material described in step 1 is hardened by work hardening, grain refinement, etc., and its hardness is greater than 150 HV.

[0100] Specifically, the high thermal conductivity material described in step 1 is high purity copper.

[0101] Specifically, the high-purity nickel material forming process described in step 2 is sampled by stamping, and the cone mouth angle of the conical structure is 120°.

[0102] Specifically, the diameters of the high-purity nickel material parts at the welding positions described in step 2 are φ26mm and φ20mm respectively, the diameters of the through-type circular holes of the high-purity copper parts at the welding positions are φ26mm and φ20mm respectively, and the large outer diameter is 76mm.

[0103] Specifically, the contact surface size matching clearance between the high-purity nickel component and the copper component described in step three is ≤0.05mm, the upper and lower surfaces are welded, the two ends of the contact surface are sealed, and the contact surface groove and protrusion combination structure is designed, the groove and protrusion width is 1.5mm, and the concave width and protrusion height are 3mm.

[0104] Specifically, step four adopts laser welding.

[0105] Specifically, the welding depth of the component welding position described in step 4 is 3 mm, the welding width is 1.5 mm, and the welding bonding rate is 99%.

[0106] The interface cone structure prepared by the method of the present invention is as follows: Figure 6 As shown, when the metal solution signal drops to 1 / 4 at a high temperature plasma temperature of 1000°C in an inductively coupled plasma mass spectrometer, the usage time is greater than 1000 hours.

[0107] Comparative Example 1:

[0108] Step 1: Provide a cone material with a melting point of >1200℃ and a high thermal conductivity material with a thermal conductivity of >90W / (m·K);

[0109] Step 2: Process the cone-shaped block material into a cone-shaped structure, and process a through circular hole in the center of the high thermal conductivity material circular plate;

[0110] Step 3: The contact surface between the cone-mouth blank component and the base blank component is processed into a high-precision matching structure, and the upper and lower welding parts are processed at the same time;

[0111] Step 4: After the contact surfaces are fitted, double-sided welding is performed on the upper and lower welding parts;

[0112] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0113] Specifically, the cone mouth material described in step 1 is a platinum alloy, and the impurity element content is less than 100ppm.

[0114] Specifically, the platinum alloy material described in step 1 is hardened by work hardening, grain refinement, etc., and has a hardness of 90 HV.

[0115] Specifically, the high thermal conductivity material described in step 1 is high purity copper.

[0116] Specifically, the platinum alloy material forming process described in step 2 is sample stamping forming, and the cone angle of the conical structure is 120°.

[0117] Specifically, the diameters of the platinum alloy material parts at the welding positions described in step 2 are φ10mm and φ8mm respectively, the diameters of the through-type circular holes of the high-purity copper parts at the welding positions are φ10mm and φ8mm respectively, and the large outer diameter is 76mm.

[0118] Specifically, the contact surface size gap between the conical material and the high thermal conductivity material described in step three is ≤0.1mm, the upper and lower surfaces are welded, the two ends of the contact surface are sealed, and the contact surface is designed as a bevel structure with a bevel angle of 45°.

[0119] Specifically, step four adopts high energy electron beam welding.

[0120] Specifically, the welding depth of the components at the welding position described in step 4 is 3 mm, the welding width is 1.5 mm, and the welding bonding rate is 90%.

[0121] The interface cone structure prepared by the method of the present invention is as follows: Figure 4 As shown, the interface cone has a low bonding rate and poor thermal conductivity due to the slope contact surface. When the metal solution signal drops to 1 / 4 at a high temperature plasma temperature of 1000° C. in an inductively coupled plasma mass spectrometer, the service life is less than 800 hours.

[0122] Comparative Example 2:

[0123] Step 1: Provide a cone material with a melting point of >1200℃ and a high thermal conductivity material with a thermal conductivity of >90W / (m·K);

[0124] Step 2: Process the cone-shaped block material into a cone-shaped structure, and process a through circular hole in the center of the high thermal conductivity material circular plate;

[0125] Step 3: The contact surface between the cone-mouth blank component and the base blank component is processed into a high-precision matching structure, and the upper and lower welding parts are processed at the same time;

[0126] Step 4: After the contact surfaces are fitted, double-sided welding is performed on the upper and lower welding parts;

[0127] Step 5: Precision machining and surface polishing are performed to obtain the finished mass spectrometer interface cone.

[0128] Specifically, the cone mouth material described in step 1 is high-purity nickel, and the content of impurity elements is less than 100ppm.

[0129] Specifically, the high-purity nickel material described in step 1 is hardened by work hardening, grain refinement, etc., and its hardness is greater than 150 HV.

[0130] Specifically, the high thermal conductivity material described in step 1 is high purity copper.

[0131] Specifically, the high-purity nickel material forming process described in step 2 is sampled by stamping forming, and the cone mouth angle of the conical structure is 120°.

[0132] Specifically, the diameters of the high-purity nickel material parts at the welding positions described in step 2 are φ26mm and φ20mm respectively, the diameters of the through-type circular holes of the high-purity copper parts at the welding positions are φ26mm and φ20mm respectively, and the large outer diameter is 76mm.

[0133] Specifically, the contact surface size matching clearance between the high-purity nickel component and the copper component in step three is ≤0.1mm, the upper and lower surfaces are welded, the two ends of the contact surface are sealed, and the contact surface has no special structural design.

[0134] Specifically, step four adopts laser welding.

[0135] Specifically, the welding depth of the components at the welding position described in step 4 is 3 mm, the welding width is 1.5 mm, and the welding bonding rate is 95%.

[0136] The interface cone structure prepared by the method of the present invention is as follows: Figure 7 As shown, due to the low bonding rate of the heterogeneous material contact surface and poor thermal conductivity, the interface cone has a service life of less than 800 hours when the metal solution signal drops to 1 / 4 at a high temperature plasma temperature of 1000°C in an inductively coupled plasma mass spectrometer.

[0137] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a mass spectrometer interface cone, characterized in that: include: The corresponding contact surfaces and upper and lower welding parts are processed on the outer periphery of the flange of the tapered blank component and the inner periphery of the circular hole of the substrate blank component to obtain the tapered component and the substrate component; The contact surfaces of the tapered part and the base part are fitted together, and double-sided welding is performed on the upper and lower welding parts.

2. The method for preparing a mass spectrometer interface cone according to claim 1, characterized in that: The matching clearance of the contact surfaces is ≤0.05mm.

3. The method for preparing a mass spectrometer interface cone according to claim 2, characterized in that: The contact surface is a special structural design for increasing the contact area, and the special structural design includes: cutting teeth, bevels, grooves or bumps.

4. The method for preparing a mass spectrometer interface cone according to claim 1, characterized in that: The cone mouth blank component is made of a cone mouth material with a melting point greater than 1200°C.

5. The method for preparing a mass spectrometer interface cone according to claim 4, characterized in that: The hardness of the cone mouth material is ≥80HV.

6. A method for preparing a mass spectrometer interface cone according to claim 4 or 5, characterized in that: The cone mouth material is a high-purity material that is resistant to high temperatures and corrosion, and the content of impurity elements is ≤100ppm.

7. The method for preparing a mass spectrometer interface cone according to claim 6, characterized in that: The cone mouth material includes: high-purity nickel, high-purity platinum and platinum alloy.

8. The method for preparing a mass spectrometer interface cone according to claim 1, characterized in that: The substrate blank component is made of a high thermal conductivity material with a thermal conductivity greater than 90 W / (m·K).

9. The method for preparing a mass spectrometer interface cone according to claim 1, characterized in that: The mass spectrometer interface cone blank component obtained after double-sided welding is subjected to precision machining and surface polishing.

10. A method for preparing a mass spectrometer interface cone according to claim 8 or 9, characterized in that: The welding techniques used for the double-sided welding include: electron beam welding and laser welding.

Citation Information

Patent Citations

  • Self-tightening conical ring sealing structure

    CN102434668A

  • Precise interface cone component and preparation method and application thereof

    CN118046178A

  • Plasma ion mass spectrometer

    JP1995161335A

  • Nozzle and skimmer for high frequency inductive coupling plasma mass spectrograph

    JP1996115702A

  • Plasma ion mass spectrometry device and method thereof

    JP2002008584A