Preparation method of self-stress high-strength sound-insulation floor
By using modified expansion agent and high-strength responsive fibers in concrete to form a communicating pore structure, combined with 3D printing technology, the problem that existing sound insulation floor materials cannot take into account sound absorption and load-bearing performance, and achieve high-efficiency sound insulation and high-strength The floor design reduces material usage and cost.
Patent Information
- Application Number
- CN202411031147.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
Existing sound insulation floor materials cannot take into account both sound absorption and load-bearing performance. The porous structure will reduce the load-bearing capacity while reducing noise efficiency. The addition of sound insulation materials may lead to a decrease in the load-bearing capacity of the floor, affecting the stability of the building.
Use modified expansion agent and high-strength responsive fiber to form a connecting pore structure in the concrete. The porous bracket is constructed through 3D printing technology, and the fibers are arranged in a directional manner during spray hydration and curing, spontaneously generate preset stress, and improve the density and strength of the concrete. Achieve uniform distribution of stress near pores.
It improves the sound insulation effect and load-bearing capacity of the floor slabs, while reducing the use and cost of materials, achieving the social needs of green and environmental protection, and solving the problem of taking into account both sound insulation and load-bearing performance.
Smart Images

Figure CN118952407A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of engineering material preparation, and specifically relates to a method for preparing a self-stressed high-strength and highly sound-insulating floor slab. Background Art
[0002] With the advancement of urban modernization, the acceleration of residential commercialization and the improvement of people's living standards, residential buildings are gradually transforming from survival-oriented to health-oriented. Floor sound insulation is one of the important guarantees of residential sound environment. Noise will not only affect hearing and sleep, but in more serious cases may also have adverse effects on people's cardiovascular system, nervous system, and endocrine system. Enhancing the sound insulation capacity of floors is one of the issues that my country's residential industry has been paying close attention to.
[0003] In order to reduce the harm of noise to the human body in daily life, sound insulation materials with good sound insulation performance are usually used in house building materials. Sound insulation materials are usually porous structures. The pore structure design is conducive to the entry of sound waves into the material, causing air vibration between the pores, thereby converting sound energy into heat energy and being absorbed. At present, the porous structure of sound insulation materials is usually prepared by foaming method, which forms unconnected pores, and the paths for sound waves to enter the material are reduced, resulting in reduced noise reduction efficiency. At the same time, directly adding sound insulation materials to load-bearing components will significantly reduce their sound insulation capabilities. In addition, the installation of sound insulation materials may cause the load-bearing capacity of the floor itself to decrease, which is not conducive to the stability requirements of the overall building.
[0004] The Chinese patent "A Prestressed Concrete Structure Decorative Integrated Sound-Absorbing Floor" (application number CN202122112316.8, publication number: CN215977982U, announcement date 2022.03.08) discloses a prestressed concrete structure decorative integrated sound-absorbing floor, which adopts a combination of decorative surface perforated plates and porous sound-absorbing materials for sound absorption, and adopts a prestressed concrete slab structure to meet the force requirements. Although the introduction of pores has been achieved, an integrated design has not been achieved, and metal connectors are required to be used to connect the various parts, which brings inconvenience to subsequent construction. Therefore, directly designing a porous interconnected pore structure in the current reinforced concrete load-bearing material to construct a porous floor with good sound insulation and excellent load-bearing capacity is a difficult problem to be solved in the field of engineering materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a self-stressed high-strength sound-insulating floor slab, so as to solve the problem that the sound-insulating floor slab materials in the prior art cannot simultaneously take into account the sound absorption and sound insulation and load-bearing performance.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a self-stressed high-strength sound-insulating floor slab is specifically implemented according to the following steps:
[0008] Step 1, prefabrication of modified expansion agent:
[0009] The expander microparticles, the precursor powder and the particle forming agent are mixed to obtain pre-particles, and the pre-particles are treated at high temperature and high pressure to obtain a modified expander;
[0010] Step 2, preparation of high-strength responsive fibers:
[0011] The modified swelling agent obtained in step 1 is added to the gel precursor solution and the fiber is immersed therein, and covalently cross-linked in an alkaline environment and under cross-linking conditions to obtain a high-strength responsive fiber;
[0012] Step 3: Construct preformed porous floor slabs:
[0013] The fibers obtained in step 2 are added to the concrete slurry, and after being fully stirred, a three-dimensional spray bonding technology is used to adjust the 3D printing parameters to print the concrete porous bracket, and the bracket is shaped at a certain temperature and humidity to obtain a preformed porous floor slab;
[0014] Step 4: Maintain the self-stressed slab:
[0015] The preformed porous floor slab obtained in step 3 is dried and then sprayed with water for curing to obtain a self-stressed, high-strength, and highly sound-insulating floor slab.
[0016] Furthermore, in step 1, the expansion agent is any one of magnesium oxide and calcium sulfoaluminate, the precursor powder is any one of inorganic calcium salts, the particle forming agent is any one of cement-based concrete adhesive and acrylic adhesive, and the mass ratio of the expansion agent microparticles, the precursor powder and the particle forming agent is 1:1:5.
[0017] Furthermore, the specific method of step 1 is: stirring and mixing the expansion agent microparticles, precursor powder and particle forming agent at a high temperature of 80-100°C for 3-5 hours, then placing them on ice for cooling to obtain pre-particles, and finally subjecting them to high temperature and high pressure treatment. The high temperature and high pressure treatment conditions are: placing them at 100-160°C under saturated water vapor pressure for 15-20 hours to obtain a modified expansion agent.
[0018] Furthermore, in step 2, the content of modified expansion agent particles is 2-4wt%; the gel precursor solution is composed of polyethylene glycol PEG, hydroxypropyl-α-cyclodextrin CD and tannic acid TA, and the molar ratio is 1:8:8; the coverage of hydroxypropyl-α-cyclodextrin on the PEG chain is 1-2%; the average molecular weight of PEG is 35,000g / mol, and the PEG is 0.18-0.38mol; the fiber is any one of an organic polymer long fiber and a metal long fiber, and the fiber diameter is 0.2-0.5mm. Furthermore, the specific method of step 2 is: adding the modified swelling agent to the gel precursor solution and immersing the fiber therein, and reacting for 2-4 hours at a temperature of 40-80°C, adjusting the alkaline environment with TRIS, the pH being 7.0-7.4, and then adding the cross-linking agent and continuing to mix for 2-4 hours. The cross-linking agent is divinyl sulfone DVS, and the cross-linking agent content is 2-4 times that of hydroxypropyl-α-cyclodextrin. Covalent cross-linking is carried out under alkaline environment and cross-linking conditions to obtain high-strength responsive fibers.
[0019] Furthermore, in step 3, the nozzle diameter of the 3D printer is 0.1-0.25 mm, the extrusion pressure is 0.4-0.6 MPa, the printing speed is set to 5-15 mm / s, the printing layer thickness is 200-400 μm, and the filling gap is 0.1-0.8 mm.
[0020] Furthermore, in step 3, the shaping conditions are: temperature of 20-25° C., humidity of 65%-85%, and drying time of 24-76 hours.
[0021] Further, in step 3, the concrete slurry is any one of cement-type concrete grouting materials;
[0022] Furthermore, in step 4, the drying conditions are: the geotextile is dried for 1-3 days; the spray hydration temperature is 30-37°C, the spray frequency is 1-3 times a day, each time for 3-6 hours, and the curing time is 7-28 days.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention prepares a interconnected pore structure on the basis of a traditional reinforced concrete structure. The formed pore structure is conducive to sound waves entering the interior of the material, causing air vibration between the pores, thereby converting sound energy into heat energy and being absorbed, thereby playing a partial insulation effect. At the same time, the slurry ejected from the 3D printing nozzle contains fibers whose length is greater than the nozzle length. The fiber directional arrangement is achieved by utilizing the shear force during ejection. During the concrete curing process, the growth of the expansion agent crystals is promoted to show the matrix expansion effect. The directional arrangement of the fibers inhibits the continued expansion of the concrete, thereby spontaneously generating a preset stress in the matrix. At the same time, the inorganic salt-modified expansion particles are used, and the ions in the inorganic calcium salt react with the ions in the cement to form a new compound to fill the microcracks in the concrete, thereby increasing the density and strength of the concrete, effectively transferring the generated prestress from the fiber to the matrix, realizing uniform distribution of concrete matrix stress near the pores, compensating for the reduced load-bearing performance due to the increase in the pore structure, and the structural design achieves a double improvement in the sound insulation effect while ensuring the engineering use requirements. In addition, the introduction of the pore structure can reduce the porosity, further reduce the amount of materials used, and reduce costs, thereby meeting the social needs of green environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A structural diagram of a self-stressed, high-strength, and highly sound-insulating floor slab prepared by the present invention;
[0026] Figure 2 This is a position relationship diagram of the three-dimensional concrete stacking structure between the steel bars and their surroundings.
[0027] In the attached figure, 1-rebar, 2-concrete three-dimensional stacking structure, 3-high-strength responsive fiber. DETAILED DESCRIPTION
[0028] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0029] The method for preparing a self-stressed high-strength and highly sound-insulating floor slab of the present invention is specifically implemented according to the following steps:
[0030] Step 1, prefabricating a modified expansion agent: mixing microparticles of an expansion agent such as magnesium oxide, calcium sulfoaluminate, etc., any inorganic calcium salt precursor powder such as calcium oxide, calcium carbonate, etc., and any particle forming agent such as a cement-based concrete adhesive, an acrylic adhesive, etc., at a mass fraction of 1:1:5 at a high temperature of 80-100°C for 3-5 hours, and then placing it on ice to cool to obtain pre-granules, and placing it at 100-160°C under saturated water vapor pressure for 15-20 hours to obtain modified expansion agent particles.
[0031] Step 2, preparing high-strength responsive fibers: adding the modified expansion agent particles (content of 2-4wt%) obtained in step 1 to the gel precursor solution and immersing any kind of fiber such as organic polymer long fibers, metal long fibers (filaments) with a diameter of 0.2-0.5mm therein, and reacting for 2-4h at a temperature of 40-80°C, adjusting the alkaline environment with TRIS to a pH of 7.0-7.4, then adding a cross-linking agent and continuing mixing for 2-4h, the cross-linking agent is divinyl sulfone (DVS), and the cross-linking agent content is 2-4 times that of hydroxypropyl-α-cyclodextrin (CD), and covalently cross-linking is performed under alkaline environment and cross-linking conditions to obtain high-strength responsive fibers.
[0032] The gel precursor solution is composed of polyethylene glycol (PEG), hydroxypropyl-α-cyclodextrin (CD) and tannic acid (TA) in a molar ratio of 1:8:8; the coverage of hydroxypropyl-α-cyclodextrin on the PEG chain is 1-2%; the average molecular weight of PEG is 35,000 g / mol, and that of PEG is 0.18-0.38 mol.
[0033] Step 3, constructing a preformed porous floor slab: adding the high-strength responsive fiber obtained in step 2 to any concrete slurry in the cement-type concrete grouting material, stirring it thoroughly, and then using three-dimensional spray bonding (3DPG) technology to adjust the 3D printing parameters to print the concrete porous bracket, and shaping it for 24-76 hours at a temperature of 20-25°C and a humidity of 65%-85% to obtain a preformed porous floor slab.
[0034] The 3D printer nozzle diameter is 0.1-0.25mm (half the fiber length), the extrusion pressure is 0.4-0.6MPa, the printing speed is set to 5-15mm / s, the printing layer thickness is 200-400μm, and the filling gap is 0.1-0.8mm;
[0035] Step 4, curing to obtain a self-stressed floor: drying the preformed porous floor covering geotextile obtained in step 3 for 1-3 days, and then curing it by spray hydration at a spray hydration temperature of 30-37°C, ensuring that the spray frequency is 1-3 times a day, each time for 3-6 hours, and curing for 7-28 days to obtain a self-stressed floor.
[0036] like Figure 1 As shown, the modified expansion agent particles obtained in step 1 are added to the gel precursor solution and the fiber is immersed therein, and the high-strength response fiber 3 is obtained after the reaction; when the 3D printing parameters are adjusted for printing, since the printing nozzle diameter is half of the fiber length, the shear force during the extrusion of the slurry forms a directional arrangement of the fiber, and the 3D printing parameters are adjusted to control the content and pore size of the slurry extruded in a single print, thereby forming a concrete three-dimensional stacking structure 2 around the steel bar 1, Figure 2The positional relationship between the steel bars 1 and the concrete three-dimensional stacking structure 2 is specifically shown.
[0037] The present invention utilizes the characteristics of good concrete fluidity and self-solidification under curing conditions. On the basis of traditional reinforced concrete structure, 3D printing technology is used to prepare interconnected pore structures in concrete. The pore structure is conducive to the entry of sound waves into the material, causing air vibration between pores, thereby converting sound energy into heat energy and being absorbed, thereby playing a partial insulation effect. The slurry sprayed out of the 3D printing nozzle contains fibers with a length greater than the nozzle length, and the fiber directional arrangement is achieved by the shear force during spraying; during the concrete curing process, the growth of the expansion agent crystal is promoted to show the matrix expansion effect, and the directional arrangement of the fibers inhibits the continued expansion of the concrete, thereby spontaneously generating preset stress in the matrix, and the ions in the inorganic salt react with the ions in the cement to form new compounds that can fill microcracks to achieve effective stress transmission, and realize the uniform distribution of concrete matrix stress near the pores, thereby compensating for the load-bearing performance reduced by the increase of local pore structure. The structural design achieves a double improvement in sound insulation effect while ensuring the requirements of engineering use. In addition, the introduction of the pore structure can reduce the porosity, further reduce the amount of materials used, and reduce costs, thereby meeting the social needs of green environmental protection.
[0038] Example 1
[0039] Magnesium oxide expansion agent microparticles, calcium oxide precursor powder and cement-based concrete binder are mixed at a mass ratio of 1:1:5 at 80°C for 3 hours, then placed on ice for cooling to obtain pre-particles, and placed at 100°C for 15 hours under saturated water vapor pressure to obtain modified expansion agent particles;
[0040] 2 wt % of the modified swelling agent particles are added to a gel precursor solution and a polylactic acid long fiber with a diameter of 0.2 mm is immersed therein, wherein the average molecular weight of PEG is 35,000 g / mol and the amount of PEG is 0.18 mol; the solution is immersed in a gel precursor composed of polyethylene glycol (PEG), hydroxypropyl-α-cyclodextrin (CD) and tannic acid (TA) in a molar ratio of 1:8:8 at a temperature of 40° C. and reacted for 2 hours, and then the pH is adjusted to 7.0 by TRIS, and divinyl sulfone (DVS) with a mass fraction of 2 times that of hydroxypropyl-α-cyclodextrin (CD) is added for cross-linking for 2 hours, thereby obtaining a coverage rate of 1% of hydroxypropyl-α-cyclodextrin on the PEG chain;
[0041] Using a printing slurry composed of cement and sand, the nozzle diameter of the 3D printer was set to 0.1 mm, the extrusion pressure was set to 0.4 MPa, the printing speed was set to 5 mm / s, the printing layer thickness was 200 μm, and the filling gap was 0.1 mm; after printing, the preformed porous floor slab was fixed at a temperature of 20°C and a humidity of 65% for 24 hours;
[0042] The preformed porous floor slab is covered with geotextile and dried for 1 day; the spray hydration temperature is set to 30°C, once a day, each time for 3 hours, and after 7 days of spray hydration curing, a self-stressed high-strength and strong sound-insulating floor slab is obtained.
[0043] Example 2
[0044] Magnesium oxide expansion agent microparticles, calcium oxide precursor powder and cement-based concrete binder are mixed at a mass ratio of 1:1:5 at 85°C for 3.5 hours, then placed on ice for cooling to obtain pre-particles, and placed at 120°C under saturated water vapor pressure for 16 hours to obtain modified expansion agent particles;
[0045] 2.5wt% of the modified expansion agent particles were added to the gel precursor solution and the polylactic acid long fiber with a diameter of 0.5mm was immersed in it, the average molecular weight of PEG was 35,000g / mol, and the PEG was 0.25mol; it was immersed in the gel precursor composed of polyethylene glycol (PEG), hydroxypropyl-α-cyclodextrin (CD) and tannic acid (TA) with a molar ratio of 1:8:8 at a temperature of 60℃ for 3h, and then the pH was adjusted to 7.2 by TRIS, and divinyl sulfone (DVS) with a mass fraction of 3 times that of hydroxypropyl-α-cyclodextrin (CD) was added for cross-linking for 3h. Thus, the coverage of hydroxypropyl-α-cyclodextrin on the PEG chain was 1.5%;
[0046] Using a printing slurry composed of cement and sand, the nozzle diameter of the 3D printer was set to 0.25 mm, the extrusion pressure was set to 0.5 MPa, the printing speed was set to 10 mm / s, the printing layer thickness was 300 μm, and the filling gap was 0.5 mm; after printing, the preformed porous floor slab was fixed at a temperature of 22°C and a humidity of 75% for 48 hours;
[0047] The preformed porous floor slab covered with geotextile was dried for 2 days; the spray hydration temperature was set to 32°C, twice a day, each time for 4 hours, and after spray hydration curing for 14 days, a self-stressed high-strength and highly sound-insulating floor slab was obtained.
[0048] Example 3
[0049] Calcium sulfoaluminate expansion agent microparticles, calcium carbonate precursor powder and acrylic adhesive are mixed at a mass ratio of 1:1:5 at 100°C for 5 hours, then placed on ice for cooling to obtain pre-particles, and placed at 160°C under saturated water vapor pressure for 20 hours to obtain modified expansion agent particles;
[0050] 3 wt % of the modified expansion agent particles are added to a gel precursor solution and a polylactic acid long fiber with a diameter of 0.5 mm is immersed therein, wherein the average molecular weight of PEG is 35,000 g / mol and the amount of PEG is 0.38 mol; the solution is immersed in a gel precursor composed of polyethylene glycol (PEG), hydroxypropyl-α-cyclodextrin (CD) and tannic acid (TA) in a molar ratio of 1:8:8 at a temperature of 80°C for 4 hours, and then the pH is adjusted to 7.4 by TRIS, and divinyl sulfone (DVS) with a mass fraction of 4 times that of hydroxypropyl-α-cyclodextrin (CD) is added for cross-linking for 4 hours, thereby obtaining a coverage rate of 2% of hydroxypropyl-α-cyclodextrin on the PEG chain;
[0051] Using a printing slurry composed of cement and sand, the nozzle diameter of the 3D printer was set to 0.25 mm, the extrusion pressure was set to 0.6 MPa, the printing speed was set to 15 mm / s, the printing layer thickness was 400 μm, and the filling gap was 0.8 mm; after printing, the preformed porous floor slab was fixed at a temperature of 25°C and a humidity of 80% for 76 hours;
[0052] The preformed porous floor slab is covered with geotextile and dried for 3 days; the spray hydration temperature is set to 35°C, 3 times a day, each time for 5 hours, and after 20 days of spray hydration curing, a self-stressed high-strength and highly sound-insulating floor slab is obtained.
[0053] Example 4
[0054] Calcium sulfoaluminate expansion agent microparticles, calcium carbonate precursor powder and acrylic adhesive were stirred and mixed at a mass ratio of 1:1:5 at 100°C for 5 hours, then placed on ice for cooling to obtain pre-particles, and placed at 160°C under saturated water vapor pressure for 20 hours to obtain modified expansion agent particles.
[0055] 4 wt% of the modified swelling agent particles are added to a gel precursor solution and a metal titanium wire (long fiber) with a diameter of 0.5 mm is immersed therein, the average molecular weight of PEG is 35,000 g / mol, and the PEG is 0.38 mol; the solution is immersed in a gel precursor composed of polyethylene glycol (PEG), hydroxypropyl-α-cyclodextrin (CD) and tannic acid (TA) in a molar ratio of 1:8:8 at a temperature of 80°C for 4 hours, and then the pH is adjusted to 7.4 by TRIS, and divinyl sulfone (DVS) with a mass fraction of 4 times that of hydroxypropyl-α-cyclodextrin (CD) is added for cross-linking for 4 hours, thereby obtaining a coverage rate of 2% of hydroxypropyl-α-cyclodextrin on the PEG chain;
[0056] Using a printing slurry composed of cement and sand, the nozzle diameter of the 3D printer was set to 0.25 mm, the extrusion pressure was set to 0.6 MPa, the printing speed was set to 15 mm / s, the printing layer thickness was 400 μm, and the filling gap was 0.8 mm; after printing, the preformed porous floor slab was fixed at a temperature of 25°C and a humidity of 80% for 76 hours;
[0057] The preformed porous floor slab is covered with geotextile and dried for 3 days; the hydration temperature is set at 37°C, spray hydration is performed 3 times a day, each time for 6 hours, and a self-stressed high-strength and strong sound-insulating floor slab is obtained after 28 days of curing.
[0058] Table 1 Comparison of load-bearing range of Examples 1-4 and 3D printed porous concrete
[0059] category Load-bearing range (kg / m2) Noise Reduction Coefficient (NRC) 3D Printing Porous Concrete 133-168 / Example 1 216.5-224 0.33 Example 2 236.3-253.8 0.57 Example 3 259.7-274.9 0.69 Example 4 270.3-294.8 0.81
[0060] Table 1 is a comparison of the bearing capacity of Examples 1-4 and 3D printed porous concrete. It can be seen from Table 1 that the self-stressed high-strength and strong sound-insulating floor slab prepared by the present invention using 3D printing technology, the addition of three-dimensional interconnecting holes improves the sound insulation capacity of the floor slab, and the self-stress design improves the bearing capacity of the floor slab itself.
[0061] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a self-stressed high-strength sound-insulating floor slab, characterized in that: Follow the steps below to implement it: Step 1, prefabrication of modified expansion agent: The expander microparticles, the precursor powder and the particle forming agent are mixed to obtain pre-particles, and the pre-particles are treated at high temperature and high pressure to obtain a modified expander; Step 2, preparation of high-strength responsive fibers: The modified swelling agent obtained in step 1 is added to the gel precursor solution and the fiber is immersed therein, and covalently cross-linked in an alkaline environment and under cross-linking conditions to obtain a high-strength responsive fiber; Step 3: Construct preformed porous floor slabs: The fibers obtained in step 2 are added to the concrete slurry, and after being fully stirred, a three-dimensional spray bonding technology is used to adjust the 3D printing parameters to print the concrete porous bracket, and the bracket is shaped at a certain temperature and humidity to obtain a preformed porous floor slab; Step 4: Maintain the self-stressed slab: The preformed porous floor slab obtained in step 3 is dried and then sprayed with water for curing to obtain a self-stressed, high-strength, and highly sound-insulating floor slab.
2. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: In step 1, the expansion agent is any one of magnesium oxide and calcium sulfoaluminate, the precursor powder is any one of inorganic calcium salts, the particle forming agent is any one of cement-based concrete adhesive and acrylic adhesive, and the mass ratio of the expansion agent microparticles, the precursor powder and the particle forming agent is 1:1:
5.
3. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: The specific method of step 1 is: stir and mix the expander microparticles, precursor powder and particle forming agent at a high temperature of 80-100°C for 3-5 hours, then place them on ice for cooling to obtain pre-particles, and finally treat them at high temperature and high pressure. The high temperature and high pressure treatment conditions are: place them at 100-160°C under saturated water vapor pressure for 15-20 hours to obtain a modified expander.
4. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: In step 2, the content of modified expansion agent particles is 2-4wt%; the gel precursor solution is composed of polyethylene glycol PEG, hydroxypropyl-α-cyclodextrin CD and tannic acid TA, and the molar ratio is 1:8:8; the coverage of hydroxypropyl-α-cyclodextrin on the PEG chain is 1-2%; the average molecular weight of PEG is 35,000g / mol, and the PEG is 0.18-0.38mol; the fiber is any one of organic polymer long fiber and metal long fiber, and the fiber diameter is 0.2-0.5mm.
5. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: The specific method of step 2 is: adding the modified swelling agent to the gel precursor solution and immersing the fiber therein, and reacting for 2-4 hours at a temperature of 40-80°C, adjusting the alkaline environment with TRIS, the pH is 7.0-7.4, and then adding the cross-linking agent and continuing to mix for 2-4 hours. The cross-linking agent is divinyl sulfone DVS, and the cross-linking agent content is 2-4 times that of hydroxypropyl-α-cyclodextrin. Covalent cross-linking is carried out under alkaline environment and cross-linking conditions to obtain high-strength responsive fibers.
6. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: In step 3, the nozzle diameter of the 3D printer is 0.1-0.25 mm, the extrusion pressure is 0.4-0.6 MPa, the printing speed is set to 5-15 mm / s, the printing layer thickness is 200-400 μm, and the filling gap is 0.1-0.8 mm.
7. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: In step 3, the shaping conditions are: temperature of 20-25° C., humidity of 65%-85%, and drying time of 24-76 hours.
8. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: In step 3, the concrete slurry is any one of cement-type concrete grouting materials.
9. The method for preparing a self-stressed high-strength and highly sound-insulating floor slab according to claim 1, characterized in that: In step 4, the drying conditions are: the geotextile is dried for 1-3 days; the spray hydration temperature is 30-37°C, the spray frequency is 1-3 times a day, each time for 3-6 hours, and the curing time is 7-28 days.
Citation Information
Cited By
Manufacturing method of micro porous structure additive added with thermal expansion graphite