Special plastic aluminum foil composite paper and preparation method thereof
By adding a special plastic layer and paper layer to the aluminum foil, combined with titanium salt solution impregnation and double-sided hot pressing technology, the problem of insufficient performance of traditional aluminum foil is solved, and the fold resistance, puncture resistance and moisture resistance are improved, and the resistance to long-term It has a service life and maintains food quality and safety in food packaging.
Patent Information
- Application Number
- CN202411027359.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Traditional aluminum foil has shortcomings in its fold resistance, flexibility, puncture resistance, moisture resistance, heat sealing properties and corrosion resistance, resulting in poor performance in food packaging and other applications, short service life, and high Performance deteriorates when exposed to corrosive media.
Special plastic aluminum foil composite paper, including aluminum foil layer, special plastic layer and paper layer, the special plastic layer is made of polyimide, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, nanomagnetic particle microcapsules and other materials The paper layer is composed of raw paper wood pulp, polyester fiber pulp, rami fiber pulp, etc., and is processed through titanium salt solution impregnation, spraying and double-sided hot pressing to form a tightly bonded layered structure.
Significantly improves the folding resistance, flexibility, puncture resistance, moisture resistance and heat sealing properties of composite paper, enhances corrosion resistance, extends service life, and maintains food quality and safety in food packaging, suitable for complex environments .
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite paper production, and in particular to a special plastic aluminum foil composite paper and a preparation method thereof. Background Art
[0002] With the rapid development of the packaging industry, the performance requirements for packaging materials are increasing. In the field of food packaging, aluminum foil has been widely used because of its good barrier properties, thermal conductivity and corrosion resistance. However, traditional aluminum foil has gradually exposed some performance defects in actual use. On the one hand, ordinary aluminum foil has poor folding resistance and flexibility. After repeated folding or bending operations, it is easy to break, delaminate and crease, which not only affects its appearance, but also reduces its performance. At the same time, the puncture resistance is limited. When facing some scenes that require higher puncture resistance, ordinary aluminum foil may be easily pierced by sharp objects, resulting in a decrease in its barrier performance and failure to effectively protect the items in the package. On the other hand, the moisture-proof performance of ordinary aluminum foil still has room for improvement. When it is in a high humidity environment for a long time or in contact with water, its moisture-proof ability will gradually weaken, and moisture may penetrate the paper, affecting the quality of the items in the package. In addition, if it is a multi-layer composite aluminum foil, the bonding strength between the layers is often insufficient, and delamination is easy to occur during use, which affects the overall performance and service life.
[0003] In addition, in applications that require heat sealing, the heat sealing performance of ordinary aluminum foil is not ideal, the heat sealing strength is insufficient or leakage is likely to occur after heat sealing. Moreover, the corrosion resistance of ordinary aluminum foil is also relatively limited. When it comes into contact with certain chemicals or corrosive media, it is prone to corrosion, which in turn affects its performance and service life. Summary of the invention
[0004] In view of this, the present invention provides a special plastic-aluminum foil composite paper and a preparation method thereof to solve the above problems.
[0005] The technical solution of the present invention is implemented as follows: a special plastic aluminum foil composite paper: comprising an aluminum foil layer, a special plastic layer, and a paper layer, wherein the aluminum foil layer is used as a base layer of the composite paper, and the special plastic layer is closely attached to one side of the aluminum foil layer, and the special plastic layer is made of the following raw materials in parts by weight: 40-60 parts of polyimide, 30-50 parts of polytetrafluoroethylene, 25-35 parts of ethylene-tetrafluoroethylene copolymer, 20-29 parts of ethylene-vinyl alcohol copolymer, and nano 12-22 parts of magnetic particle microcapsules, the paper layer is combined with the other side opposite to the special plastic layer, and the paper layer is made of the following raw materials in parts by weight: 50-80 parts of base paper pulp, 15-22 parts of polyester fiber pulp, 10-20 parts of ramie fiber pulp, 10-20 parts of reel fiber pulp, 5-12 parts of rosin glue, 20-30 parts of chitin, 5-8 parts of chitosan, 2-4 parts of allicin, and 1-3 parts of propolis. The base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
[0006] Furthermore, the aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 1-20 μm.
[0007] Furthermore, the nano magnetic particle microcapsule comprises the following percentage raw materials: 40-50% magnetic nanoparticles, 10-30% capsule core material, 2-4% monomer, 1-10% emulsifier, and the balance is water. The magnetic nanoparticles are ferroferric oxide, ferric oxide particles, and cobalt nanoparticles, and the particle size is 1-100nm.
[0008] Furthermore, the capsule core material is liquid paraffin, olive oil and vegetable oil in a mass ratio of (12-15):(20-30):(3-8).
[0009] Furthermore, the monomer is selected from styrene or acrylonitrile.
[0010] Furthermore, the emulsifier is selected from alkylphenol polyoxyethylene ether, sodium lauryl sulfate or dodecyltrimethylammonium bromide.
[0011] Furthermore, the nano-magnetic particle microcapsule is prepared by mixing magnetic nano-particles with a capsule core material, stirring for 20-40 minutes to form a magnetic capsule core emulsion, and mixing the magnetic capsule core emulsion with a monomer and water under the action of an emulsifier, and irradiating the mixture under γ-rays for 5-8 hours, wherein the γ-ray radiation dose is 0.2-30 KGy and the dose rate is 0.3-10 Gy / s to form a microcapsule with magnetic properties.
[0012] Furthermore, the paper layer is prepared by mixing and beating base paper pulp, polyester fiber pulp, ramie fiber pulp, and reel fiber pulp at 90-120° C. and 2000-3000 rpm to obtain pulp I; mixing rosin glue, chitin, chitosan, allicin, and propolis, and stirring at 4000-6000 rpm to obtain pulp II; mixing the above pulp I and pulp II uniformly and performing electrophoretic deposition for 20-40 minutes, controlling the voltage to 50-100 V, and the current to 10-100 mA / cm 2 , forming paper materials, and papermaking forms paper layers with an ordered layered structure.
[0013] Furthermore, a method for preparing a special plastic-aluminum foil composite paper comprises the following steps:
[0014] S1. Surface pretreatment of the aluminum foil layer: impregnation of the aluminum foil with a titanium salt solution having a mass concentration of 80-90%, the impregnation temperature being 40-80°C, and the impregnation time being 10-15 minutes;
[0015] S2, preparing special plastics: mixing and stirring polyimide, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, ethylene-vinyl alcohol copolymer, and nano-magnetic particle microcapsules to obtain special plastics;
[0016] S3. Apply special plastic layer: spray the special plastic onto the surface of the aluminum foil layer, the spray gun pressure is 0.5-0.8MPa, the spray distance is 10-25cm, the coating flow rate is 3-20g / min, the spray gun speed is 0.1-1m / s, and the spray temperature is 15-30℃;
[0017] S4, coating the paper layer: combining the paper layer with one side of the special plastic, and hot pressing the laminated aluminum foil layer-special plastic layer-paper layer on both sides for 20-30 minutes at a temperature of 150-250° C. and a pressure of 120-150 KN to obtain a special plastic aluminum foil composite paper.
[0018] Furthermore, a special plastic-aluminum foil composite paper is used in the field of food packaging.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] Significantly improved folding resistance and flexibility: Through the optimized combination and preparation process of each layer of materials, the composite paper is not easy to break, delaminate or crease when repeatedly folded and bent, and can better adapt to different shapes and packaging requirements, improve performance and extend service life.
[0021] Enhanced puncture resistance: The addition of materials such as nano-magnetic particle microcapsules and the synergistic effect of each layer structure enable the composite paper to withstand puncture from sharp objects, maintain good barrier properties, and better protect the items in the package.
[0022] Improved moisture-proof performance: The characteristics and close combination of each layer of material enable the composite paper to effectively prevent moisture penetration in a high humidity environment or when in contact with water, providing a stable dry environment for the internal items.
[0023] Good composite fastness: The layers are processed by specific process and combined with materials, with high bonding strength. It is not easy to delaminate during use, ensuring the overall stable performance of the composite paper.
[0024] Improved heat sealing performance: The optimized composite paper has high heat sealing strength, good sealing after heat sealing, and is not prone to leakage, meeting the requirements of heat sealing performance for food packaging.
[0025] Enhanced corrosion resistance: When exposed to chemicals or corrosive media, it can maintain stable performance and reduce the impact of corrosion on the performance of composite paper, making it suitable for various complex use environments.
[0026] When used in the field of food packaging, it can effectively maintain the quality and safety of food, extend the shelf life of food, and has broad market application prospects and commercial value. DETAILED DESCRIPTION
[0027] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0028] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0029] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0030] Example 1
[0031] A special plastic aluminum foil composite paper: comprising an aluminum foil layer, a special plastic layer, and a paper layer, wherein the aluminum foil layer serves as a base layer of the composite paper;
[0032] The aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 1-20 μm;
[0033] The special plastic layer is closely attached to one side of the aluminum foil layer, and the special plastic layer is made of the following raw materials in parts by weight: 40 parts of polyimide, 30 parts of polytetrafluoroethylene, 25 parts of ethylene-tetrafluoroethylene copolymer, 20 parts of ethylene-vinyl alcohol copolymer, and 12 parts of nano-magnetic particle microcapsules;
[0034] The nano magnetic particle microcapsules are prepared by mixing magnetic nano particles with capsule core materials, stirring for 20 minutes to form a magnetic capsule core emulsion, mixing the magnetic capsule core emulsion with monomers and water under the action of an emulsifier, and irradiating under gamma rays for 5 hours, wherein the gamma ray radiation dose is 0.2 KGy and the dose rate is 0.3 Gy / s, to form microcapsules with magnetic properties.
[0035] The paper layer is combined with the other side opposite to the special plastic layer, and the paper layer is made of the following raw materials in parts by weight: 50 parts of base paper pulp, 15 parts of polyester fiber pulp, 10 parts of ramie fiber pulp, 10 parts of reel fiber pulp, 5 parts of rosin glue, 20 parts of chitin, 5 parts of chitosan, 2 parts of allicin, and 1 part of propolis. The base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
[0036] The paper layer is prepared by mixing and beating base paper pulp, polyester fiber pulp, ramie fiber pulp and reel fiber pulp at 90° C. and 2000 rpm to obtain pulp I; rosin glue, chitin, chitosan, allicin and propolis are mixed and stirred at 4000 rpm to obtain pulp II; the pulp I and pulp II are mixed and electrophoretically deposited for 20 minutes, and the voltage is controlled to be 50 V and the current is 10 mA / cm 2 , forming paper materials, and papermaking forms paper layers with an ordered layered structure.
[0037] Example 2
[0038] A special plastic aluminum foil composite paper: comprising an aluminum foil layer, a special plastic layer, and a paper layer, wherein the aluminum foil layer serves as a base layer of the composite paper;
[0039] The aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 20 μm;
[0040] The special plastic layer is closely attached to one side of the aluminum foil layer, and the special plastic layer is made of the following raw materials in parts by weight: 60 parts of polyimide, 50 parts of polytetrafluoroethylene, 35 parts of ethylene-tetrafluoroethylene copolymer, 29 parts of ethylene-vinyl alcohol copolymer, and 22 parts of nano-magnetic particle microcapsules;
[0041] The nano magnetic particle microcapsule is prepared by mixing magnetic nano particles with capsule core materials, stirring for 40 minutes to form a magnetic capsule core emulsion, mixing the magnetic capsule core emulsion with monomers and water under the action of an emulsifier, and irradiating under gamma rays for 8 hours, wherein the gamma ray radiation dose is 30 KGy and the dose rate is 10 Gy / s, to form a microcapsule with magnetic properties.
[0042] The paper layer is combined with the other side opposite to the special plastic layer, and the paper layer is made of the following raw materials in parts by weight: 80 parts of base paper pulp, 22 parts of polyester fiber pulp, 20 parts of ramie fiber pulp, 20 parts of reel fiber pulp, 12 parts of rosin glue, 30 parts of chitin, 8 parts of chitosan, 4 parts of allicin, and 3 parts of propolis. The base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
[0043] The paper layer is prepared by mixing and beating base paper pulp, polyester fiber pulp, ramie fiber pulp and reel fiber pulp at 120° C. and 3000 rpm to obtain pulp I; mixing rosin glue, chitin, chitosan, allicin and propolis, and stirring at 6000 rpm to obtain pulp II; mixing the above pulp I and pulp II evenly and performing electrophoretic deposition for 40 minutes, with a control voltage of 100 V and a current of 100 mA / cm 2 , forming paper materials, and papermaking forms paper layers with an ordered layered structure.
[0044] Example 3
[0045] A special plastic aluminum foil composite paper: comprising an aluminum foil layer, a special plastic layer, and a paper layer, wherein the aluminum foil layer serves as a base layer of the composite paper;
[0046] The aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 15 μm;
[0047] The special plastic layer is closely attached to one side of the aluminum foil layer, and the special plastic layer is made of the following raw materials in parts by weight: 50 parts of polyimide, 40 parts of polytetrafluoroethylene, 30 parts of ethylene-tetrafluoroethylene copolymer, 25 parts of ethylene-vinyl alcohol copolymer, and 17 parts of nano-magnetic particle microcapsules;
[0048] The nano magnetic particle microcapsules are prepared by mixing magnetic nano particles with capsule core materials, stirring for 30 minutes to form a magnetic capsule core emulsion, mixing the magnetic capsule core emulsion with monomers and water under the action of an emulsifier, and irradiating under γ rays for 7 hours, wherein the γ ray radiation dose is 15 KGy and the dose rate is 5 Gy / s, to form microcapsules with magnetic properties.
[0049] The paper layer is combined with the other side opposite to the special plastic layer, and the paper layer is made of the following raw materials in parts by weight: 70 parts of base paper pulp, 18 parts of polyester fiber pulp, 15 parts of ramie fiber pulp, 15 parts of reel fiber pulp, 8 parts of rosin glue, 25 parts of chitin, 7 parts of chitosan, 3 parts of allicin, and 2 parts of propolis. The base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
[0050] The paper layer is prepared by mixing and beating base paper pulp, polyester fiber pulp, ramie fiber pulp and reel fiber pulp at 100° C. and 2500 rpm to obtain pulp I; rosin glue, chitin, chitosan, allicin and propolis are mixed and stirred at 5000 rpm to obtain pulp II; the pulp I and pulp II are mixed and electrophoretically deposited for 30 minutes, and the voltage is controlled to be 80 V and the current is 50 mA / cm 2 , forming paper material, and making paper layers with orderly layered structure;
[0051] The above examples 1-3 adopt the following preparation method:
[0052] S1. Surface pretreatment of the aluminum foil layer: the aluminum foil is impregnated with a titanium salt solution having a mass concentration of 85%, the impregnation temperature is 60° C., and the impregnation time is 12 min;
[0053] S2, preparing special plastics: mixing and stirring polyimide, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, ethylene-vinyl alcohol copolymer, and nano-magnetic particle microcapsules to obtain special plastics;
[0054] S3. Apply special plastic layer: spray the special plastic onto the surface of the aluminum foil layer, with a spray gun pressure of 0.7 MPa, a spray distance of 15 cm, a coating flow rate of 15 g / min, a spray gun speed of 0.5 m / s, and a spray temperature of 22°C;
[0055] S4, coating the paper layer: combining the paper layer with one side of the special plastic, and hot pressing the laminated aluminum foil layer-special plastic layer-paper layer on both sides at a temperature of 200° C. and a pressure of 130 KN for 25 minutes to obtain a special plastic aluminum foil composite paper.
[0056] Example 4
[0057] A special plastic aluminum foil composite paper: comprising an aluminum foil layer, a special plastic layer, and a paper layer, wherein the aluminum foil layer serves as a base layer of the composite paper;
[0058] The aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 15 μm;
[0059] The special plastic layer is closely attached to one side of the aluminum foil layer, and the special plastic layer is made of the following raw materials in parts by weight: 50 parts of polyimide, 40 parts of polytetrafluoroethylene, 30 parts of ethylene-tetrafluoroethylene copolymer, 25 parts of ethylene-vinyl alcohol copolymer, and 17 parts of nano-magnetic particle microcapsules;
[0060] The nano magnetic particle microcapsules are prepared by mixing magnetic nano particles with capsule core materials, stirring for 30 minutes to form a magnetic capsule core emulsion, mixing the magnetic capsule core emulsion with monomers and water under the action of an emulsifier, and irradiating under γ rays for 7 hours, wherein the γ ray radiation dose is 15 KGy and the dose rate is 5 Gy / s, to form microcapsules with magnetic properties.
[0061] The paper layer is combined with the other side opposite to the special plastic layer, and the paper layer is made of the following raw materials in parts by weight: 70 parts of base paper pulp, 18 parts of polyester fiber pulp, 15 parts of ramie fiber pulp, 15 parts of reel fiber pulp, 8 parts of rosin glue, 25 parts of chitin, 7 parts of chitosan, 3 parts of allicin, and 2 parts of propolis. The base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
[0062] The paper layer is prepared by mixing and beating base paper pulp, polyester fiber pulp, ramie fiber pulp and reel fiber pulp at 100° C. and 2500 rpm to obtain pulp I; rosin glue, chitin, chitosan, allicin and propolis are mixed and stirred at 5000 rpm to obtain pulp II; the pulp I and pulp II are mixed and electrophoretically deposited for 30 minutes, and the voltage is controlled to be 80 V and the current is 50 mA / cm 2 , forming paper material, and making paper layers with orderly layered structure;
[0063] The above-mentioned Example 4 adopts the following preparation method:
[0064] S1. Surface pretreatment of the aluminum foil layer: impregnation of the aluminum foil with a titanium salt solution having a mass concentration of 80-90%, the impregnation temperature being 40° C., and the impregnation time being 10 min;
[0065] S2, preparing special plastics: mixing and stirring polyimide, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, ethylene-vinyl alcohol copolymer, and nano-magnetic particle microcapsules to obtain special plastics;
[0066] S3. Apply special plastic layer: spray the special plastic onto the surface of the aluminum foil layer, with a spray gun pressure of 0.5 MPa, a spray distance of 10 cm, a coating flow rate of 3 g / min, a spray gun speed of 0.1 m / s, and a spray temperature of 15°C;
[0067] S4, coating the paper layer: combining the paper layer with one side of the special plastic, and hot pressing the laminated aluminum foil layer-special plastic layer-paper layer on both sides for 20 minutes at a temperature of 150° C. and a pressure of 120 KN to obtain a special plastic aluminum foil composite paper.
[0068] Example 5
[0069] A special plastic aluminum foil composite paper: comprising an aluminum foil layer, a special plastic layer, and a paper layer, wherein the aluminum foil layer serves as a base layer of the composite paper;
[0070] The aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 15 μm;
[0071] The special plastic layer is closely attached to one side of the aluminum foil layer, and the special plastic layer is made of the following raw materials in parts by weight: 50 parts of polyimide, 40 parts of polytetrafluoroethylene, 30 parts of ethylene-tetrafluoroethylene copolymer, 25 parts of ethylene-vinyl alcohol copolymer, and 17 parts of nano-magnetic particle microcapsules;
[0072] The nano magnetic particle microcapsules are prepared by mixing magnetic nano particles with capsule core materials, stirring for 30 minutes to form a magnetic capsule core emulsion, mixing the magnetic capsule core emulsion with monomers and water under the action of an emulsifier, and irradiating under γ rays for 7 hours, wherein the γ ray radiation dose is 15 KGy and the dose rate is 5 Gy / s, to form microcapsules with magnetic properties.
[0073] The paper layer is combined with the other side opposite to the special plastic layer, and the paper layer is made of the following raw materials in parts by weight: 70 parts of base paper pulp, 18 parts of polyester fiber pulp, 15 parts of ramie fiber pulp, 15 parts of reel fiber pulp, 8 parts of rosin glue, 25 parts of chitin, 7 parts of chitosan, 3 parts of allicin, and 2 parts of propolis. The base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
[0074] The paper layer is prepared by mixing and beating base paper pulp, polyester fiber pulp, ramie fiber pulp and reel fiber pulp at 100° C. and 2500 rpm to obtain pulp I; rosin glue, chitin, chitosan, allicin and propolis are mixed and stirred at 5000 rpm to obtain pulp II; the pulp I and pulp II are mixed and electrophoretically deposited for 30 minutes, and the voltage is controlled to be 80 V and the current is 50 mA / cm 2 , forming paper material, and making paper layers with orderly layered structure;
[0075] The above-mentioned Example 5 adopts the following preparation method:
[0076] S1. Surface pretreatment of the aluminum foil layer: the aluminum foil is impregnated with a titanium salt solution having a mass concentration of 90%, the impregnation temperature is 80°C, and the impregnation time is 15 minutes;
[0077] S2, preparing special plastics: mixing and stirring polyimide, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, ethylene-vinyl alcohol copolymer, and nano-magnetic particle microcapsules to obtain special plastics;
[0078] S3. Apply special plastic layer: spray the special plastic onto the surface of the aluminum foil layer, with a spray gun pressure of 0.8 MPa, a spray distance of 25 cm, a coating flow rate of 20 g / min, a spray gun speed of 1 m / s, and a spray temperature of 30°C;
[0079] S4, coating the paper layer: combining the paper layer with one side of the special plastic, and hot pressing the laminated aluminum foil layer-special plastic layer-paper layer on both sides for 30 minutes at a temperature of 250° C. and a pressure of 150 KN to obtain a special plastic aluminum foil composite paper.
[0080] Comparative Example 1
[0081] The difference between this comparative example and implementation 3 is that the special plastic layer is made of the following raw materials in parts by weight: 70 parts of polyimide, 25 parts of polytetrafluoroethylene, 20 parts of ethylene-tetrafluoroethylene copolymer, 18 parts of ethylene-vinyl alcohol copolymer, and 10 parts of nano-magnetic particle microcapsules.
[0082] Comparative Example 2
[0083] The difference between this comparative example and implementation 3 is that the raw material of the special plastic layer does not contain nano magnetic particle microcapsules.
[0084] Comparative Example 3
[0085] The difference between this comparative example and implementation 3 is that the paper layer is made of the following raw materials in parts by weight: 40 parts of base paper pulp, 25 parts of polyester fiber pulp, 8 parts of ramie fiber pulp, 25 parts of reel fiber pulp, 3 parts of rosin glue, 35 parts of chitin, 2 parts of chitosan, 5 parts of allicin, and 5 parts of propolis.
[0086] Test Example 1-Effect Test
[0087] The special plastic aluminum foil composite papers prepared in the above Examples 1-5 and Comparative Examples 1-3 were used as 10 groups of samples for testing:
[0088] 1. Folding resistance test:
[0089] Randomly select at least 5 samples from the plastic-aluminum foil composite paper samples to be tested, each with a size of 150mm×15mm; clamp the samples vertically on the clamp of the MIT folding endurance tester so that the folding part of the sample is located in the middle of the clamp. Set the folding angle of the MIT folding endurance tester to 135° and the folding speed to 175 times / minute. Start the instrument and begin to fold the samples repeatedly, and record the number of folds of each sample when it breaks.
[0090] 2. Flexibility test:
[0091] Randomly select at least 5 specimens from the plastic-aluminum foil composite paper samples to be tested, each with a size of 200mm×25mm. Fix one end of the specimen and place the other end horizontally on the cylindrical shaft of the cylindrical shaft bending test device. Bend the specimen 180° around the cylindrical shaft evenly at a speed of 2-3s, and observe whether there are cracks, fractures or delamination on the surface of the specimen. Start with the cylindrical shaft with a larger diameter, gradually replace the cylindrical shaft with a smaller diameter, and repeat the above bending operation until the specimen is damaged, and record the diameter of the cylindrical shaft at this time.
[0092] 3. Puncture resistance
[0093] According to the relevant requirements of "6.6.13 Puncture Strength" in "GB / T10004-2008 Plastic Composite Film, Bag Dry Composite, Extrusion Composite for Packaging"; use a sampler to cut 5 circular samples with a diameter of 100mm from the surface of the plastic aluminum foil composite paper, ensure that the sample thickness is uniform, without wrinkles, folds, stains and other obvious defects, and puncture the sample at a speed of (50±5)mm / min; when the puncture needle penetrates the sample, the test machine will automatically stop and record the maximum load value. Repeat the above steps until all samples are tested.
[0094] 4. Data Results
[0095] Folding times (times) Flexible diameter(mm) Puncture resistance(N) Example 1 5205 6 14 Example 2 5120 7 14 Example 3 5320 6 15 Example 4 5100 6 13 Example 5 5050 8 12 Comparative Example 1 3460 15 5 Comparative Example 2 3450 17 6 Comparative Example 3 3350 17 7
[0096] The above results show that the embodiment group is significantly better than the comparative example group in terms of folding resistance, flexibility and puncture resistance. The process and material combination of the embodiment group makes the plastic aluminum foil composite paper have significant advantages in mechanical properties and performance, and can better meet the application requirements with higher product performance requirements.
[0097] Comparison between Example 3 and Comparative Examples 1 and 3 shows that the raw materials of the special plastic layer and the paper layer can achieve better effects in a certain ratio.
[0098] Compared with Comparative Example 2, Example 3 shows that the nano-magnetic particle microcapsules are evenly dispersed in the plastic layer, which can disperse stress when subjected to external force and prevent rapid crack expansion, thereby improving the toughness and impact resistance of the plastic-aluminum foil composite paper.
[0099] Test Example 2-Corrosion Test
[0100] Set the following comparison ratio:
[0101] Comparative Example 4
[0102] The difference between this comparative example and implementation 3 is that the paper layer raw material does not contain allicin.
[0103] Comparative Example 5
[0104] The difference between this comparative example and implementation 3 is that the paper layer raw material does not contain propolis.
[0105] Example 3 and Comparative Examples 4 and 5 were selected as test samples, and their mass loss rate and appearance changes were tested within 24 hours by immersing them in a corrosive medium of 5% hydrochloric acid solution and 10% sodium hydroxide solution, respectively.
[0106] Mass loss rate = (initial mass - final mass) / initial mass × 100%
[0107] The results are as follows:
[0108] Table 2: Corrosion resistance test results in acidic environment (5% hydrochloric acid solution)
[0109] Mass loss rate (%) Description of appearance changes Example 3 0.30 Slight discoloration, no flaking Comparative Example 4 0.89 Darker color, slightly peeled edges Comparative Example 5 0.75 Local darkening of the surface
[0110] Table 3: Corrosion resistance test results in alkaline environment (10% sodium hydroxide solution)
[0111] Mass loss rate (%) Description of appearance changes Example 3 0.04 Almost no change Comparative Example 4 0.35 Slight gloss reduction Comparative Example 5 0.44 Glossiness is significantly reduced, no peeling
[0112] From the above results, it can be seen that, compared with Example 4, allicin as a raw material for the paper layer in Example 3 can capture and neutralize oxidizing substances in the environment (such as oxygen, ozone, etc.), reduce the erosion of the composite paper by the oxidation reaction, and delay the aging and corrosion process of the paper layer and the composite paper as a whole; allicin molecules can form an adsorption film on the surface of the aluminum foil to block the direct contact between corrosive media (such as moisture, oxygen, corrosive ions, etc.) and the metal surface, thereby playing a certain role in corrosion inhibition and protection of the aluminum foil layer.
[0113] Compared with Comparative Example 5, in Example 3, propolis is used as the raw material for the paper layer, and the active ingredients therein react chemically with the surface of the aluminum foil to form a stable protective film on the surface of the aluminum foil, thereby preventing direct interaction between the aluminum foil and the corrosive medium and slowing down the rate of the electrochemical corrosion reaction, thereby providing corrosion protection for the aluminum foil layer. The antioxidant components such as phenols and flavonoids in propolis can capture and neutralize free radicals in the environment, reduce the damage of the oxidation reaction to the organic components in the composite paper (such as the polymer materials in the plastic layer and the paper layer), delay the aging and corrosion process of the composite paper, and maintain the performance and structural stability of the composite paper.
[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A special plastic-aluminum foil composite paper, characterized by: The invention comprises an aluminum foil layer, a special plastic layer and a paper layer, wherein the aluminum foil layer serves as a base layer of the composite paper, the special plastic layer is closely attached to one side of the aluminum foil layer, the special plastic layer is made of the following raw materials in parts by weight: 40-60 parts of polyimide, 30-50 parts of polytetrafluoroethylene, 25-35 parts of ethylene-tetrafluoroethylene copolymer, 20-29 parts of ethylene-vinyl alcohol copolymer and 12-22 parts of nano magnetic particle microcapsules, the paper layer is combined with the other side opposite to the special plastic layer, the paper layer is made of the following raw materials in parts by weight: 50-80 parts of base paper pulp, 15-22 parts of polyester fiber pulp, 10-20 parts of ramie fiber pulp, 10-20 parts of reel fiber pulp, 5-12 parts of rosin glue, 20-30 parts of chitin, 5-8 parts of chitosan, 2-4 parts of allicin and 1-3 parts of propolis, and the base paper pulp is selected from coniferous wood pulp or broadleaf wood pulp.
2. The special plastic-aluminum foil composite paper according to claim 1, characterized in that: The aluminum foil layer is an aluminum foil with a purity of more than 99.5% and a thickness of 1-20 μm.
3. The special plastic-aluminum foil composite paper according to claim 1, characterized in that: The nano magnetic particle microcapsule comprises the following raw materials in percentage: 40-50% magnetic nanoparticles, 10-30% capsule core material, 2-4% monomer, 1-10% emulsifier, and the balance is water. The magnetic nanoparticles are ferroferric oxide, ferric oxide particles, and cobalt nanoparticles, and the particle size is 1-100nm.
4. The special plastic-aluminum foil composite paper according to claim 3, characterized in that: The capsule core material is liquid paraffin, olive oil and vegetable oil in a mass ratio of (12-15):(20-30):(3-8).
5. The special plastic-aluminum foil composite paper according to claim 3, characterized in that: The monomer is selected from styrene or acrylonitrile.
6. The special plastic-aluminum foil composite paper according to claim 3, characterized in that: The emulsifier is selected from alkylphenol polyoxyethylene ether, sodium lauryl sulfate or dodecyltrimethylammonium bromide.
7. The special plastic-aluminum foil composite paper according to claim 3, characterized in that: The nano magnetic particle microcapsules are prepared by mixing magnetic nano particles with capsule core materials, stirring for 20-40 minutes to form a magnetic capsule core emulsion, mixing the magnetic capsule core emulsion with monomers and water under the action of an emulsifier, and irradiating under gamma rays for 5-8 hours, wherein the radiation dose of the gamma rays is 0.2-30 KGy and the dose rate is 0.3-10 Gy / s to form microcapsules with magnetism.
8. The special plastic-aluminum foil composite paper according to claim 1, characterized in that: The paper layer is prepared by mixing and beating base paper wood pulp, polyester fiber pulp, ramie fiber pulp and reel fiber pulp at 90-120° C. and 2000-3000 rpm to obtain pulp I; mixing rosin glue, chitin, chitosan, allicin and propolis, and stirring at 4000-6000 rpm to obtain pulp II; mixing the above pulp I and pulp II evenly and performing electrophoretic deposition for 20-40 minutes, controlling the voltage to 50-100 V and the current to 10-100 mA / cm 2 , forming paper materials, and papermaking forms paper layers with an ordered layered structure.
9. The method for preparing a special plastic-aluminum foil composite paper according to claim 1, characterized in that: The following steps are involved: S1. Surface pretreatment of the aluminum foil layer: impregnation of the aluminum foil with a titanium salt solution having a mass concentration of 80-90%, the impregnation temperature being 40-80°C, and the impregnation time being 10-15 minutes; S2, preparing special plastics: mixing and stirring polyimide, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, ethylene-vinyl alcohol copolymer, and nano-magnetic particle microcapsules to obtain special plastics; S3. Apply special plastic layer: spray the special plastic onto the surface of the aluminum foil layer, the spray gun pressure is 0.5-0.8MPa, the spray distance is 10-25cm, the coating flow rate is 3-20g / min, the spray gun speed is 0.1-1m / s, and the spray temperature is 15-30℃; S4, coating the paper layer: combining the paper layer with one side of the special plastic, and hot pressing the laminated aluminum foil layer-special plastic layer-paper layer on both sides for 20-30 minutes at a temperature of 150-250° C. and a pressure of 120-150 KN to obtain a special plastic aluminum foil composite paper.
10. Application of the special plastic-aluminum foil composite paper according to any one of claims 1 to 9 in the field of food packaging.
Citation Information
Patent Citations
Aluminium-plastic film and preparation method for same
CN103158298A
Composite structure and production method therefor, packaging material and molded article using same, and coating liquid
CN103958078A
Fragrance slow-release type damp-proof aluminum foil lining paper and preparation method thereof
CN112195684A
Transfer material, recorded matter, method of manufacturing recorded matter, image-recording apparatus, and apparatus for manufacturing recorded matter
US20160288535A1
Aluminum-plastic composite film and preparation method therefor
WO2024119460A1