Method for separating selenium and tellurium from copper anode slime

By using catalysts and redox agents in copper anode mud, combined with alkali and acid leaching treatment, the problems of low selenium-tellurium separation efficiency and low precious metal recovery are solved, and efficient and low-cost selenium-tellurium separation and precious metal recovery are achieved. Improves product purity and environmental friendliness.

CN118954439APending Publication Date: 2024-11-15ZHEJIANG HONGDA METAL SMELTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411005741.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing selenium-tellurium separation process has low efficiency, especially for high tellurium crude selenium raw materials, which are not good at separation. The traditional process has high requirements for equipment, high cost, unfriendly environment, and low precious metal recovery rate and low product purity.

Method used

Using sulfur dioxide to oxidize active metal under catalyst conditions in copper anode mud, add alkali and acid leaching to improve the solubility and purity of selenium tellurium, and improve the separation degree of selenium tellurium and the recovery rate of precious metals through multiple recycling steps. The sulfide salt removes metal ions to improve product purity.

Benefits of technology

It improves the separation purity and yield of selenium tellurium, reduces the loss and production cost of precious metals, simplifies the operation process, realizes efficient selenium tellurium separation and precious metal recycling, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962966120000061
    Figure BDA0004962966120000061
  • Figure BDA0004962966120000071
    Figure BDA0004962966120000071
  • Figure BDA0004962966120000072
    Figure BDA0004962966120000072
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgy, in particular to a method for separating selenium and tellurium from copper anode slime. The method for separating selenium and tellurium from the copper anode slime comprises the following steps: S1, separating selenium and tellurium; s2, oxidizing and alkaline leaching; S3, adjusting the pH value; S4, recycling selenium; and S5, recycling for multiple times. According to the technical scheme, the method has the advantages that selenium and tellurium are separated from the liquid obtained after gold immersion, meanwhile, the recovery rate of precious metal in the liquid obtained after gold immersion is higher, and meanwhile the separation degree and yield of selenium and tellurium are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metallurgical technology, and in particular to a method for separating selenium and tellurium from copper anode mud. Background Art

[0002] Selenium and tellurium are commonly used in sensors and infrared optical materials, pigments, and high-tech industries such as semiconductor equipment, optoelectronic equipment, and solar cells. They play an increasingly important role in the national economy, and market demand continues to increase.

[0003] The mainstream traditional process is oxygen oxidation, which is to produce selenium dioxide by oxidizing and burning crude selenium raw materials. Selenium dioxide is soluble in water to form selenious acid, and ammonia water is used to adjust the pH to 4-5 to remove tellurium. This process route has a long wet process, high equipment requirements, high cost, and the intermediate finished product selenium dioxide is a hazardous chemical, which is not environmentally friendly; the vacuum distillation method uses the different vapor pressures and evaporation rates of selenium, tellurium and impurity elements at the same temperature to control a certain temperature and vacuum degree to volatilize and selectively condense selenium, tellurium and impurity elements, so as to separate selenium, tellurium and impurity elements and finally obtain refined selenium, but the main problem is that the condensation coefficients of selenium and tellurium are similar, which makes them difficult to separate, and for high-tellurium crude selenium raw materials, the separation efficiency of selenium and tellurium obtained by vacuum distillation is not high. The regional smelting method is based on the difference in solubility of selenium and tellurium in the solid state and the molten state, and locally heats a narrow and long solid ingot to form a narrow melting zone and slowly move the melting zone. The distribution of impurities is controlled during the partial melting and solidification of the selenium ingot to achieve the purpose of impurity removal, but this method is inefficient and selenium and tellurium are easy to volatilize at high temperatures, making it more difficult to separate high-tellurium crude selenium raw materials. Therefore, the existing selenium-tellurium process has low separation efficiency and selenium-tellurium mixtures are difficult to separate.

[0004] The Chinese invention patent with patent number CN103172038B discloses a method for separating and purifying selenium and tellurium, which mainly purifies selenium through vacuum distillation. However, the equipment and process are not adaptable to crude selenium raw materials, especially the crude selenium raw materials from the Kaldo furnace process, which contain impurity Te content (0.28%~0.32%), which is 16 times lower than the crude selenium raw materials produced by the copper anode mud sulfuric acid roasting process (Te~0.02%). Faced with the technical demand of directly producing refined selenium from industrial-grade crude selenium, it is difficult to solve the separation of selenium and tellurium.

[0005] Chinese patent CN104743526A discloses a process for refining crude selenium, which comprises washing the crude selenium raw material with water at a weight ratio of 1:1 for 2-3 times, adding 3-8m3 of a sodium sulfite solution with a concentration of 150-300g / l to each ton of filtered residue, heating the solution to 95-100°C and reacting for 2-3h, then adding ammonium sulfide to the solution until no precipitation is produced, filtering and discarding the residue, cooling the filtrate at room temperature for 48h, and then precipitating refined selenium from the sodium sulfite solution, and adding 3-8m3 of a sodium sulfite solution with a concentration of 150-300g / l to each ton of filtered residue. 15-20 kg of washed filter residue is added to the cubic meter solution after the refined selenium is precipitated, and the precipitated refined selenium is washed until the pH value of the eluate is 7.0-7.5, and after drying, a selenium ingot with a grade of 99.99% is cast. The sodium sulfite solution that has been recycled for 5-7 times in the process can be acid-lyzed and regenerated and recycled after adding concentrated sulfuric acid for acid hydrolysis; the process of the present invention is simple, the raw material consumption is small, the production cost is low, it is environmentally friendly, the raw material adaptability is strong, and it has good economic and social benefits. The disadvantages of this scheme are that the crude selenium raw material and the sodium sulfite solution are leached, the selenium powder is difficult to dissolve, the leaching rate is not high, and for the high-tellurium crude selenium raw material, the wet separation effect is general, and the raw material adaptability is not strong. Summary of the invention

[0006] In order to separate selenium and tellurium from the post-gold precipitation liquid and achieve a higher recovery rate for the precious metals in the post-gold precipitation liquid, and to improve the separation degree and yield of selenium and tellurium, the present application provides a method for separating selenium and tellurium from copper anode mud.

[0007] The present application provides a method for separating selenium and tellurium from copper anode mud, comprising the following steps: S1: Separation of selenium and tellurium: Add deionized water to the gold precipitation liquid, add catalyst, stir at 60r / min to form a uniform suspension, continue to introduce SO2, continue stirring for 2-4 hours after the ventilation is completed, filter to remove metal powder, and vacuum dry the filtrate to obtain a crude selenium and tellurium mixture; S2: oxidative alkali leaching: add hydrogen peroxide and alkaline solution to the selenium-tellurium mixture obtained in step S1, and continue stirring at 60 r / min for 1-3 hours. After the reaction, add sulfide salt and continue stirring for 0.5-1 hour. After the reaction, filter to remove solid precipitate, and vacuum dry the filtrate to obtain a selenium-tellurium mixture product; S3: Adjusting pH: Soaking the selenium-tellurium mixture obtained in step S2 in dilute hydrochloric acid for 2-3 hours, filtering to obtain a filtrate and a filter cake, washing the filter cake several times with a 0.1 mol / L sodium hydroxide solution, and then washing with deionized water and drying to obtain a tellurium compound; S4: Selenium recovery: adding a reducing agent to the filtrate obtained in step S3, continuously stirring the reaction for 0.5-1 hour, filtering to obtain a filter cake, and vacuum drying the filter cake to obtain selenium; S5: Multiple recovery: The filtrate obtained in step S4 is vacuum concentrated and then filtered to obtain a filter cake, and the steps of S3 and S4 are repeated multiple times on the filter cake to obtain tellurium compounds and selenium.

[0008] By adopting the above technical scheme, when the traditional process treats the post-gold precipitation liquid, iron powder is generally added to the post-gold precipitation liquid to replace the selenium, tellurium, gold, platinum and palladium therein. However, in order to make the metal ions be replaced more thoroughly, excessive iron powder will be added, so that the iron powder content in the product obtained by the iron powder replacement method is high and the precious metal grade is low, which is easy to cause the loss of precious metals when the gold, platinum and palladium are recovered later, and the cost is high and the benefit is low. In this technical scheme, sulfur dioxide is introduced into the post-gold precipitation liquid under catalytic conditions. Sulfur dioxide relies on its oxidizing property to oxidize the more active copper, silver, lead, iron and other metals into metal ions and remain in the solution, while inactive metals such as gold, platinum and palladium do not participate in the reaction and remain in a solid state, so that the precious metals can be obtained by simple separation operation later. Compared with the traditional iron powder replacement method, this technical scheme has a higher recovery rate for gold, platinum and palladium precious metals while having a lower cost. At the same time, the operation is simpler and has better practicality in large-scale processing processes.

[0009] After the separation of precious metals, a large number of active metal ions are still retained in the solution. In the traditional process, selenium and tellurium are directly separated, so that the separated selenium and tellurium contain more impurities and the product purity is low. The present technical solution adds a filtrate treatment step, by adding sulfide salts to the filtrate to remove metal ions, so that in the subsequent separation process, the influence of metal ions on selenium and tellurium is reduced, thereby improving the purity of the final product.

[0010] The present application uses a method of first alkali leaching and then acid leaching when separating selenium and tellurium. In the alkali leaching process, selenium and tellurium are first oxidized by hydrogen peroxide to generate an aqueous solution of selenium and tellurium, thereby increasing the solubility of selenium and tellurium in the solution, so that the loss of selenium and tellurium can be reduced in the subsequent filtration step. In the acid leaching process, the tellurium compound is precipitated by adjusting the pH. The tellurium compound obtained in this way has a high purity. The remaining mother liquor is used to reduce the selenium compound in the solution by a reducing agent, and the selenium is reduced to a single substance and separated. The selenium and tellurium obtained by this scheme have high purity and yield.

[0011] After alkaline leaching, acid leaching and reduction processes, some selenium and tellurium still remain in the mother liquor. Through repeated treatments, as much selenium and tellurium as possible can be recovered. Compared with traditional separation processes, the separation scheme used in this application not only has a higher recovery rate of precious metals, but also the separation of selenium and tellurium is more thorough and the operation is simpler.

[0012] In the present invention, the catalyst in step S1 is one or a combination of sodium chloride, hydrochloric acid, a hydrochloric acid solution of sodium chloride and a sulfuric acid solution of sodium chloride.

[0013] By adopting the above technical scheme, in the present application, when catalytic oxidation of active metals is carried out, chloride ions play the main catalytic role. Therefore, using sodium chloride and hydrochloric acid as catalysts has a better catalytic effect. At the same time, if chloride ions want to have a better catalytic effect, they need to be catalyzed in an acidic environment. Therefore, the present application adds relatively stable sulfuric acid to provide an acidic environment, which improves the catalytic effect while reducing safety risks.

[0014] In the present invention, the molar concentration of the catalyst in step S1 is 1-1.5 mol / L.

[0015] By adopting the above technical scheme, the operators found through multiple experiments that when the catalyst concentration in the solution in step S1 is 1-1.5 mol / L, it has a good catalytic effect. When the catalyst concentration is greater than 1.5 mol / L, the catalytic effect is not greatly improved. Therefore, the molar concentration of the catalyst in the present application is preferably 1-1.5 mol / L.

[0016] In the present invention, the alkaline solution in step S2 is one or a combination of sodium hydroxide, potassium hydroxide and sodium carbonate.

[0017] By adopting the above technical solution, sodium hydroxide, potassium hydroxide and sodium carbonate can provide stronger acidity to improve the oxidation effect of hydrogen peroxide on selenium and tellurium.

[0018] In the present invention, the concentration of the hydrogen peroxide in step S2 is 200-300 mL / L, and the concentration of the alkaline solution in step S2 is 4-8 mol / L.

[0019] By adopting the above technical solution, the operators found through multiple experiments that when the concentration of the hydrogen peroxide in step S2 is 200-300mL / L, it has a good oxidation effect, and when the concentration of the alkaline solution in step S2 is 4-8mol / L, the oxidation effect of the hydrogen peroxide is stronger.

[0020] In the present invention, the sulfide salt in step S2 is one or a combination of sodium sulfide, potassium sulfide and ammonium sulfide.

[0021] By adopting the above technical scheme, sodium sulfide, potassium sulfide and ammonium sulfide are added to the solution, so that the metal ions in the solution react with the sulfide ions to form sulfide precipitates, thereby facilitating the removal of metal ions. Sodium ions and potassium ions have high solubility in water, and ammonium ions are easily removed by heating, which has little effect on the subsequent separation process. Therefore, in the present application, sodium sulfide, potassium sulfide and ammonium sulfide are more economical to use as sulfide salts.

[0022] In the present invention, the concentration of the hydrochloric acid solution in step S3 is 0.1-0.5 mol / L.

[0023] By adopting the above technical solution, since the tellurium compound easily reacts with hydrochloric acid in the highly acidic hydrochloric acid, the yield of tellurium decreases, and therefore it is necessary to use dilute hydrochloric acid with a lower concentration.

[0024] In the present invention, the solid-liquid ratio of the crude selenium-tellurium mixture to the alkaline solution in step S2 is 1:(5-10), and the solid-liquid ratio of the refined selenium-tellurium mixture to dilute hydrochloric acid in step S3 is 1:(5-10).

[0025] By adopting the above technical solution, it was found through multiple experiments that when the solid-liquid ratio of the crude selenium-tellurium mixture to the alkaline solution is 1:(5-10) and the solid-liquid ratio of the fine selenium-tellurium mixture to dilute hydrochloric acid is 1:(5-10), the leaching rate is high.

[0026] In the present invention, the catalyst in step S4 is one or a combination of sulfur dioxide, sodium sulfite, sodium bisulfite and an acid solution of sodium hypochlorite.

[0027] By adopting the above technical solution, sulfur dioxide, sodium sulfite, sodium bisulfite and sodium hypochlorite are selected as reducing agents, which not only has a strong reducing effect, but also reduces the introduction of new impurities, which is more suitable in this application.

[0028] In the present invention, the number of repetitions in step S5 is 1-2 times.

[0029] By adopting the above technical scheme, the operators found through multiple experiments that when the operation is repeated 1-2 times, the yield of selenium tellurium increases significantly. When the number of repeated experiments is greater than 3 times, the selenium tellurium remaining in the mother liquor is extremely low, and the benefit of continuing to repeat the operation is too low. Therefore, the number of repeated operations in this application is more appropriate to be 1-2 times.

[0030] In summary, the present application includes at least one of the following beneficial technical effects: 1. In this technical solution, sulfur dioxide is introduced into the liquid after gold precipitation under catalyst conditions. Sulfur dioxide relies on its oxidizing property to oxidize the more active metals such as copper, silver, lead, and iron into metal ions and remain in the solution, while inactive metals such as gold, platinum, and palladium do not participate in the reaction and remain in a solid state, so that the precious metals can be obtained through simple separation operations later, and the recovery rate of gold, platinum, and palladium precious metals is relatively high.

[0031] 2. The technical solution adds a filtrate treatment step, by adding sulfide salts to the filtrate to remove metal ions, so that the influence of metal ions on selenium and tellurium is reduced in the subsequent separation process, thereby improving the purity of the final product.

[0032] 3. In the separation of selenium and tellurium, the present application adopts a method of first alkali leaching and then acid leaching. The selenium and tellurium obtained by this scheme have high purity and yield. DETAILED DESCRIPTION

[0033] The present application is further described in detail below in conjunction with the specific contents. Example

[0034] Preparation of post-gold precipitation liquid: Copper anode mud is mixed with concentrated sulfuric acid with a weight ratio of 80% to 110%, and roasted at a temperature of 300 to 600°C. Selenium, tellurium compounds or elements in the material react chemically with sulfuric acid, and selenium volatilizes into the flue gas in the form of SeO2. A cascade water absorption tower is used to absorb SeO2 to dissolve it to generate H2SeO3, which is then reduced to amorphous red selenium by SO2 in the flue gas. The selenium precipitate in the absorption tower tank is taken out, and the liquid remaining in the absorption tower is the post-gold precipitation liquid.

[0035] Example 1 A method for separating selenium and tellurium from copper anode mud comprises the following steps: S1: Separation of selenium and tellurium: Add 100ml of the gold precipitation liquid to 100ml of deionized water, add 12g of sodium chloride and 20ml of 1mol / L hydrochloric acid solution, stir at a speed of 60r / min for half an hour to form a uniform suspension, and continue to pass SO2 for 1 hour. After the ventilation is completed, continue to stir for 2 hours, filter to remove the metal powder, and vacuum dry the filtrate to obtain a crude selenium and tellurium mixture; S2: Oxidation alkali leaching: Add 80g of 250ml / L hydrogen peroxide and 20g of 5mol / L sodium hydroxide solution to the selenium and tellurium mixture obtained in step S1, continue to stir and react at 60r / min for 2 hours, add sodium sulfide after the reaction is completed and continue to stir for 0.5 hours, filter to remove the solid precipitate after the reaction is completed, and vacuum dry the filtrate to obtain a fine selenium and tellurium mixture; S3: Adjusting pH: Soaking the selenium-tellurium mixture obtained in step S2 in 100 ml of 0.1 mol / L dilute hydrochloric acid for 2 hours, filtering to obtain a filtrate and a filter cake, washing the filter cake several times with a 0.1 mol / L sodium hydroxide solution, and then washing with deionized water and drying to obtain a tellurium compound; S4: Recovery of selenium: add 30 g of sodium bisulfite and 50 ml of 0.1 mol / L dilute sulfuric acid to the filtrate obtained in step S3, continue stirring and reacting for 0.5 hours, filter to obtain a filter cake, and vacuum dry the filter cake to obtain selenium; S5: Multiple recovery: The filtrate obtained in step S4 is vacuum concentrated and then filtered to obtain a filter cake, and steps S3 and S4 are repeated twice on the filter cake to obtain tellurium compounds and selenium. The obtained tellurium compounds and selenium are mixed with the tellurium compounds obtained in step S3 and the selenium obtained in step S4, and the total yield is calculated.

[0036] The difference between Example 2-4 and Example 1 is that the catalyst used in step S1 is different, as shown in the following table: catalyst Example 1 Sodium chloride, hydrochloric acid Example 2 Sodium chloride Example 3 hydrochloric acid Example 4 Sodium chloride, sulfuric acid The difference between Examples 5, 6 and Comparative Examples 1 and 2 and Example 1 is that the alkaline solutions used in step S2 are different, as shown in the following table: Alkali Example 1 Sodium hydroxide Example 5 Potassium hydroxide Example 6 Sodium carbonate Comparative Example 1 Sodium bicarbonate Comparative Example 2 ammonia The difference between Comparative Example 3 and Example 1 is that no sulfide salt is added in step S2.

[0037] The difference between Comparative Example 4 and Example 1 is that the conventional process is used to recover the precious metal in the gold precipitation solution in step S1, and the specific steps are as follows: Add 100 ml of gold precipitation liquid into 100 ml of deionized water, add 20 g of iron powder, and continue stirring at a speed of 60 r / min for 3 hours to form a uniform suspension. After stirring, filter to obtain metal powder. Add hydrochloric acid solution to the metal powder to remove the iron powder. After the reaction is complete, add sodium hydroxide to adjust the pH to neutral, and filter to obtain the precious metal.

[0038] The difference between Example 7 and Comparative Examples 5 and 6 and Example 1 is that the number of repetitions in step S5 is different, as shown in the following table: Number of recycling times Example 1 2 Example 7 1 Comparative Example 5 3 Comparative Example 6 4 Comparative Example 7 0 Performance testing The purity and yield of the products obtained in each embodiment and comparative example were calculated as follows: Purity: The product of each example and comparative example was dissolved in a corresponding solvent and titrated to calculate the purity of the product.

[0039] Yield: Calculate the corresponding yield based on the purity of the product.

[0040] The test results are shown in the following table: Conclusion: It can be seen from the data of Example 1 and Comparative Example 4 in the above table that in the present application, the precious metals are recovered by sulfur dioxide oxidation instead of the iron powder replacement method in the traditional process, and the recovery rate is greatly increased, and basically all the precious metals can be recovered. This is because in the traditional iron powder replacement method, when the iron powder replaces the precious metals in the gold precipitation liquid, it will also replace some metals with weaker activity, so that the filtered metal powder contains more impurities. In the subsequent process of removing iron powder and other metals, it will further lead to the loss of precious metals, resulting in a low yield of precious metals. In the present application, sulfur dioxide is added under acidic adjustment. Sulfur dioxide has a strong oxidizing property in an acidic environment, and can oxidize some inactive metals into ions and remain in the solution, while the less active precious gold, platinum and palladium still exist in a solid form. The precious metals can be easily recovered by filtration, and at the same time, a higher yield is achieved.

[0041] Conclusion: It can be seen from the data of Examples 1-4 in the above table that the catalyst in step S1 of the present application is more suitable to be a mixture of sodium chloride and hydrochloric acid. This is because the main catalytic effect in the present application is chloride ions, and chloride ions have a stronger catalytic effect in an acidic environment. Selenium-tellurium mixture fine product yield (%) Example 1 95 Example 5 91 Example 6 92 Comparative Example 1 85 Comparative Example 2 83

[0042] Conclusion: It can be seen from the data of Examples 1, 5, 6 and Comparative Examples 1 and 2 in the above table that the alkaline solution selected in step S2 of the present application is more appropriately sodium hydroxide solution. This is because in order to achieve a higher yield in the present application, a stronger alkaline environment needs to be provided, so it is more appropriate to use sodium hydroxide solution. The yield of Example 5 is lower than that of Example 1 because the solubility of the selenium-tellurium mixture in potassium hydroxide solution is higher than that in sodium hydroxide solution, which reduces the final yield. Purity of Selenium Tellurium Mixture (%) Selenium-tellurium mixture fine product yield (%) Example 1 99.5 95 Comparative Example 3 86.3 94

[0043] Conclusion: It can be seen from the data of Example 1 and Comparative Example 3 in the above table that the addition of sulfide salt in step S2 in the present application can greatly improve the purity of the product. This is because by adding sulfide salt to the solution, the metal ions in the solution react with the sulfide ions to form sulfide precipitates, thereby facilitating the removal of metal ions and thus improving the purity of the product.

[0044] Conclusion: It can be seen from the data of Examples 1, 7 and Comparative Examples 5, 6, and 7 in the above table that when the number of repeated recovery is 1-2 times, the yield is significantly improved compared to not performing repeated recovery. This is because there are still more selenium and tellurium elements remaining in the mother liquor. When the number of repetitions exceeds 2 times, the yield improvement does not change much, and there is little meaning in continuing to perform repeated recovery. Therefore, in this application, the number of repeated recovery is preferably 1-2 times.

[0045] The above-mentioned specific implementation examples are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for separating selenium and tellurium from copper anode mud, characterized in that: The steps include: S1: Separation of selenium and tellurium: Add deionized water to the gold precipitation liquid, add catalyst, stir at 60r / min to form a uniform suspension, continue to introduce SO2, continue stirring for 2-4 hours after the ventilation is completed, filter to remove metal powder, and vacuum dry the filtrate to obtain a crude selenium and tellurium mixture; S2: oxidative alkali leaching: add hydrogen peroxide and alkaline solution to the selenium-tellurium mixture obtained in step S1, and continue stirring at 60 r / min for 1-3 hours. After the reaction, add sulfide salt and continue stirring for 0.5-1 hour. After the reaction, filter to remove solid precipitate, and vacuum dry the filtrate to obtain a selenium-tellurium mixture product; S3: Adjusting pH: Soaking the selenium-tellurium mixture obtained in step S2 in dilute hydrochloric acid for 2-3 hours, filtering to obtain a filtrate and a filter cake, washing the filter cake several times with a 0.1 mol / L sodium hydroxide solution, and then washing with deionized water and drying to obtain a tellurium compound; S4: Selenium recovery: adding a reducing agent to the filtrate obtained in step S3, continuously stirring the reaction for 0.5-1 hour, filtering to obtain a filter cake, and vacuum drying the filter cake to obtain selenium; S5: Multiple recovery: The filtrate obtained in step S4 is vacuum concentrated and then filtered to obtain a filter cake, and the steps of S3 and S4 are repeated multiple times on the filter cake to obtain tellurium compounds and selenium.

2. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The catalyst in step S1 is one or a combination of sodium chloride, hydrochloric acid, a hydrochloric acid solution of sodium chloride and a sulfuric acid solution of sodium chloride.

3. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The molar concentration of the catalyst in step S1 is 1-1.5 mol / L. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that the alkaline solution in step S2 is one or a combination of sodium hydroxide, potassium hydroxide and sodium carbonate.

4. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The concentration of the hydrogen peroxide in step S2 is 200-300 mL / L, and the concentration of the alkaline solution in step S2 is 4-8 mol / L.

5. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The sulfide salt in step S2 is one or a combination of sodium sulfide, potassium sulfide and ammonium sulfide.

6. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in step S3 is 0.1-0.5 mol / L.

7. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: In the step S2, the solid-liquid ratio of the crude selenium-tellurium mixture to the alkaline solution is 1:(5-10), and in the step S3, the solid-liquid ratio of the refined selenium-tellurium mixture to the dilute hydrochloric acid is 1:(5-10).

8. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The catalyst in step S4 is one or a combination of sulfur dioxide, sodium sulfite, sodium bisulfite and an acid solution of sodium hypochlorite.

9. The method for separating selenium and tellurium from copper anode mud according to claim 1, characterized in that: The number of repetitions in step S5 is 1-2 times.

Citation Information

Patent Citations

  • Method for separating and recycling selenium and tellurium from copper anode mud

    CN106477533A

  • Method for efficiently separating selenium and tellurium from acid liquid

    CN112960654A