Process for purifying battery-grade lithium hydroxide monohydrate by solvent-out crystallization method
Through the dissolution crystallization method, the problems of reducing purity and increasing time cost caused by impurity embedding and recrystallization in the traditional lithium hydroxide purification process are solved, and a high-purity, low-energy consumption and low-cost lithium hydroxide purification process is realized. The process is also The process is environmentally friendly.
Patent Information
- Application Number
- CN202411317562.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
In the traditional lithium hydroxide purification process, impurity embedding during the crystallization and precipitation process leads to a decrease in product purity, and recrystallization increases time cost and production cycle.
By evaporation crystallization, the lithium hydroxide raw material is dissolved by mixing deionized water with solvate, stirring evenly, and evaporation crystallization, cooling and separation, agitation and suction filtration operations, combined with rinsing and drying, high purity is obtained. The lithium hydroxide crystallization product is recovered and the production cost is reduced by recycling low boiling point solectants.
A higher lithium hydroxide purity (99.87%) is achieved, reducing energy consumption and production cycles, while reducing production costs and wastewater emissions.
Smart Images

Figure CN118954548A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium hydroxide purification and preparation, and specifically relates to a battery-grade lithium hydroxide monohydrate purification process. Background Art
[0002] As an important lithium compound, lithium hydroxide is widely used in battery materials, petroleum, metallurgy, glass and ceramics industries due to its unique physical and chemical properties. It also plays an important role in national defense, military and aerospace fields. Lithium hydroxide is used to manufacture synthetic fiber rubber and other chemicals, and is an important part of lithium-ion battery electrolyte. At the same time, with the continuous development of science and technology, lithium hydroxide is increasingly used in medicine and pesticides.
[0003] Traditional lithium hydroxide purification adopts multiple evaporation crystallization method, where lithium hydroxide is mixed with deionized water and dissolved at high temperature, filtered under reduced pressure to remove insoluble impurities, and then concentrated and cooled to crystallize to obtain high-purity lithium hydroxide. This method has the advantages of repeated recycling of filtrate, high lithium yield, simple operation, and low production cost. However, in the process of crystallizing lithium hydroxide, other impurities will be embedded in the particles and precipitated together, resulting in reduced purity of the product. At the same time, the recrystallization process will also increase the time cost and extend the production cycle.
[0004] Therefore, it is of great practical significance to develop a lithium hydroxide purification process with lower energy consumption, fewer processes and higher purity. Summary of the invention
[0005] The purpose of the present invention is to provide a new battery-grade lithium hydroxide purification process to address the problems existing in the existing lithium hydroxide purification process technology, so as to achieve the goals of lower energy consumption, higher yield and purity of the lithium hydroxide purification process.
[0006] To this end, the present invention provides the following technical solution: a process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization, comprising the following steps:
[0007] Step 1: Mix deionized water and a solvent according to a certain ratio, and stir to obtain a solvent;
[0008] Step 2: using the solvent obtained in step 1 to dissolve the lithium hydroxide raw material, placing the obtained solution A in an evaporator for staged evaporation and crystallization, and obtaining a solid solution mixture of the lithium hydroxide solution according to a set concentration ratio;
[0009] Step 3, cooling the lithium hydroxide solid solution mixture obtained in step 2 to room temperature, and performing separation operation to obtain a crystalline product B and a filtrate C;
[0010] Step 4: adding a mixed solvent in a corresponding proportion to the crystalline product B obtained in step 3 to perform stirring and washing operations to obtain a solid solution mixture of lithium hydroxide again;
[0011] Step 5: filtering and separating the lithium hydroxide solid solution mixture obtained in step 4 to obtain a crystalline product D and a filtrate E;
[0012] Step six, use a dissolving agent in proportion to elute the crystalline product D, and dry to obtain the desired crystalline product; at the same time, in the entire process of preparing battery-grade lithium hydroxide by the dissolution crystallization method, the filtrate E obtained in the process can be collected and concentrated again and dissolved and crystallized to improve the overall yield of the process; at the same time, the low-boiling point dissolving agent can also be recycled by distillation.
[0013] Preferably, the solvent in step 1 should be a solvent that is miscible with the original solvent but incompatible with the solute, so as to significantly reduce the solubility of the solute in the original solvent, thereby achieving the effect of crystallization.
[0014] The solvent can be selected as an ethanol solution, and its concentration can be selected as 75% ethanol solution, 95% ethanol solution and anhydrous ethanol. The mass ratio of the solvent to deionized water is 1: (1-10)
[0015] Preferably, in step 2, the mass ratio of the solvent to the industrial lithium hydroxide raw material is (5-10):1, the dissolving stirring speed is 300-700 r / min, and the temperature is 50-60°C.
[0016] Preferably, the evaporator in step 2 is a round-bottom evaporation container.
[0017] Preferably, the evaporative crystallization in step 2 is performed by water bath rotary evaporation.
[0018] Preferably, the rotary evaporation operation in step 2 uses a segmented temperature; wherein the water bath temperature of the first segment is 30-40°C, and the water bath temperature of the second segment is 60-75°C.
[0019] Preferably, the first water bath time in step 2 is 5-10 min, and the second water bath time is 60-100 min.
[0020] Preferably, the absolute pressure inside the rotary evaporator in step 2 is maintained at about 40-100 hPa.
[0021] Preferably, the first-stage rotary evaporation speed of the round-bottom evaporator in step 2 is 40-60 r / min, and the second-stage rotary evaporation speed is 60-100 r / min.
[0022] Preferably, the concentration ratio set in step 2 is a mass ratio of the crystallized product in the solid solution mixture to the concentrated mother liquor of 1:(1.5-2).
[0023] Preferably, the cooling operation in step three uses oil bath cooling, the temperature of the oil bath is controlled at 20-30°C, and the stirring speed is 200-500r / min.
[0024] Preferably, the separation operation in step three is performed by suction filtration.
[0025] Preferably, the solvent in step 4 is an ethanol solution, the solvent solubility is 70% ethanol solution, 95% ethanol solution or anhydrous ethanol as the solvent, and the mass ratio of the solvent to deionized water is 1: (1-5)
[0026] Preferably, the stirring and washing operation in step 4 is carried out in an oil bath at a constant temperature of 20-30°C and a stirring speed of 200-500r / min.
[0027] Preferably, the stirring time in step 4 is 2-4 hours.
[0028] Preferably, the separation operation in step five is performed by suction filtration.
[0029] Preferably, in step six, a dissolving agent is used in the elution operation, and the mass ratio of the dissolving agent to the crystalline product obtained by filtration is 1:(4-6).
[0030] Preferably, the drying operation in step six can be performed by vacuum drying, with a temperature of 70-100° C., an oven pressure of 10-30 Pa, and a drying time of 12-24 h.
[0031] The purity of the lithium hydroxide finally obtained by drying is 99.87%, wherein the contents of Na and Ka are ≤5ppm, and the content of Cl is ≤5ppm.
[0032] Compared with the prior art, the technical solution provided by the present invention has the following gain effects:
[0033] (1) The battery-grade lithium hydroxide purification process of the present invention adopts the method of dissolution crystallization, utilizes the difference in molecular interaction forces between the separated solute and the solvent, and selects a dissolution agent with stronger interaction forces with the solvent, thereby reducing the solubility of the separated solute in the solvent, thereby greatly improving the yield of lithium hydroxide.
[0034] (2) The solvent used in the present invention has the advantage of being easy to recycle and can greatly reduce production costs. It is also environmentally friendly and has low wastewater discharge in the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The present invention is a lithium hydroxide purification process flow chart.
[0036] Figure 2 It is the lithium hydroxide purified product of the present invention.
[0037] Figure 3 It is the XRD diagram of the purified lithium hydroxide product of the present invention. Specific implementation methods
[0039] See also Figure 1 The present invention aims to further purify industrial-grade lithium hydroxide raw materials to meet the market demand for the purity of battery-grade lithium hydroxide raw materials. The present invention uses deionized water as a solvent to dissolve the lithium hydroxide raw material, obtains a lithium hydroxide solid solution mixture of the target ratio by vacuum rotary evaporation, and obtains a crystalline product and a saturated filtrate by suction filtration and separation. The saturated filtrate is cooled to room temperature, and a corresponding proportion of ethanol dissolution agent is added, and the mixture is stirred continuously at a constant temperature for 2-4 hours to obtain a solid solution mixture crystallized by dissolution, and the next step of crystalline product and filtrate is obtained by suction filtration and separation. The obtained crystalline product is eluted and filtered with a corresponding proportion of ethanol, and then dried to obtain a battery-grade lithium hydroxide product.
[0040] The process of the present invention is further described below with reference to specific examples.
[0041] Example 1
[0042] A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization method comprises the following steps:
[0043] (1) Use a 500 ml round-bottom flask as a container, weigh 137.5 ml of anhydrous ethanol and 137.5 ml of deionized water, and stir continuously at room temperature until the solution is mixed evenly.
[0044] (2) Add 35 g of industrial grade lithium hydroxide raw material to the solution, raise the oil bath temperature to 40° C., and continue stirring until the lithium hydroxide raw material is completely dissolved to obtain solution A.
[0045] (2) Solution A was transferred to a rotary evaporator, wherein the water bath temperature of the first stage was set to 30°C, the rotary evaporation time was 5 min, and the rotation speed was 40 r / min; the water bath temperature of the second stage was set to 60°C, the rotary evaporation time was 80 min, and the rotation speed was 80 r / min; the absolute pressure inside the device was 100 hPa, and the solid solution mixture after rotary evaporation was cooled to 30°C in an oil bath, and the solid solution mixture obtained by rotary evaporation was separated by suction filtration to obtain a crystalline product B and a filtrate C.
[0046] (3) Deionized water and a solvent are mixed in a ratio of 2:1 to obtain a stirring solution, and the crystallized product B and the stirring solution are stirred in a ratio of 1:1, and stirred at a constant temperature of 30°C for 2 hours to obtain a solid solution mixed product, and the crystallized product D and the filtrate E are separated by suction filtration.
[0047] (5) The obtained crystalline product D and the solvent are eluted in a ratio of 5:1, and after filtration, the crystalline product is transferred to a vacuum oven and dried at 80° C. for 12 h to obtain a purified lithium hydroxide product. The purified product is as follows: Figure 2 The XRD pattern of the purified product is shown in Figure 3 shown.
[0048] Example 2
[0049] A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization method comprises the following steps:
[0050] (1) Use a 500 ml round-bottom flask as a container, weigh 137.5 ml of anhydrous ethanol and 137.5 ml of deionized water, and stir continuously at room temperature until the solution is mixed evenly.
[0051] (2) Add 35 g of industrial grade lithium hydroxide raw material to the solution, raise the oil bath temperature to 40° C., and continue stirring until the lithium hydroxide raw material is completely dissolved to obtain solution A.
[0052] (2) Solution A was transferred to a rotary evaporator, wherein the first-stage water bath temperature was set to 35°C, the rotary evaporation time was 8 min, and the rotation speed was 50 r / min; the second-stage water bath temperature was set to 70°C, the rotary evaporation time was 80 min, and the rotation speed was 80 r / min; the absolute pressure inside the device was 100 hPa, and the solid solution mixture after rotary evaporation was cooled to 30°C in an oil bath, and the solid solution mixture obtained by rotary evaporation was separated by suction filtration to obtain a crystalline product B and a filtrate C.
[0053] (3) Deionized water and a solvent were mixed at a ratio of 1:1 to obtain a stirring solution, and the crystallized product B and the stirring solution were stirred at a ratio of 1:1.5, and stirred at a constant temperature of 30°C for 2 h to obtain a solid solution mixed product, and the crystallized product D and the filtrate E were separated by suction filtration.
[0054] (5) The obtained crystalline product D and the solvent are eluted in a ratio of 5:1, and after filtration, the crystalline product is transferred to a vacuum oven and dried at 80° C. for 12 h to obtain a purified lithium hydroxide product.
[0055] Example 3
[0056] A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization method comprises the following steps:
[0057] (1) Use a 500 ml round-bottom flask as a container, weigh 137.5 ml of anhydrous ethanol and 137.5 ml of deionized water, and stir continuously at room temperature until the solution is mixed evenly.
[0058] (2) Add 35 g of industrial grade lithium hydroxide raw material to the solution, raise the oil bath temperature to 40° C., and continue stirring until the lithium hydroxide raw material is completely dissolved to obtain solution A.
[0059] (2) Solution A is transferred to a rotary evaporator, wherein the first-stage water bath temperature is set to 40°C, the rotary evaporation time is 10 min, and the rotation speed is 60 r / min; the second-stage water bath temperature is set to 80°C, the rotary evaporation time is 80 min, and the rotation speed is 80 r / min; the absolute pressure inside the device is 100 hPa, and the solid solution mixture product after rotary evaporation is cooled to 30°C in an oil bath, and the solid solution mixture obtained by rotary evaporation is separated by suction filtration to obtain a crystalline product B and a filtrate C.
[0060] (3) Deionized water and a solvent are mixed in a ratio of 2:1 to obtain a stirring solution, and the crystallized product B and the stirring solution are stirred in a ratio of 1:1, and stirred at a constant temperature of 30°C for 2 hours to obtain a solid solution mixed product, and the crystallized product D and the filtrate E are separated by suction filtration.
[0061] (5) The obtained crystalline product D and the solvent are eluted in a ratio of 5:2, and after filtration, the crystalline product is transferred to a vacuum oven and dried at a constant temperature of 80° C. for 12 h to obtain a purified lithium hydroxide product.
[0062] Comparative Example
[0063] The present invention illustrates a traditional lithium hydroxide evaporation crystallization purification method
[0064] (1) Using a 500 ml round-bottom flask as a container, weigh 35 g of industrial-grade lithium hydroxide raw material and dissolve it in 200 ml of deionized water. Heat the oil bath to 50° C. and stir continuously until it is completely dissolved.
[0065] (2) The solution was transferred to an evaporation container for rotary evaporation. The round-bottom flask was heated in a water bath at 70°C. The rotation of the flask was set at 80 r / min. At the same time, the entire device was evacuated and the absolute pressure of the system was maintained at around 100 hPa.
[0066] (3) After rotary evaporation for 40 min, the obtained solid solution mixture was cooled and stirred at room temperature until the crystallization was completely precipitated;
[0067] (4) The obtained solid solution mixture is filtered to obtain a crystalline product, which is transferred into a vacuum oven and dried at 80° C. for 12 h to obtain a purified lithium hydroxide product.
[0068] The content of the battery-grade lithium hydroxide product obtained by purifying battery-grade lithium hydroxide monohydrate by the dissolution crystallization method of the present invention is measured below.
[0069] Table 1 Battery grade lithium hydroxide monohydrate D-1 content standard and Example 1-3, comparative example content determination
[0070]
[0071] As shown in Table 1, the battery-grade lithium hydroxide product obtained by the process of purifying battery-grade lithium hydroxide monohydrate by the dissolution crystallization method of the present invention can meet the standard requirements of battery-grade lithium hydroxide monohydrate D-1 level. However, it can be seen from the comparative examples that only the ordinary rotary evaporation cooling crystallization operation cannot meet the requirements of battery-grade lithium hydroxide monohydrate.
[0072] Obviously, the above examples of the present invention are only used as illustrations to explain the present invention, and are not intended to limit the methods of the present invention. All obvious extensions or changes made on the basis of the present invention are within the scope of protection of the present invention.
Claims
1. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization, characterized in that: The process steps include: Step 1: Mix deionized water and a solvent according to a certain ratio, and stir to obtain a solvent; Step 2: using the solvent obtained in step 1 to dissolve the lithium hydroxide raw material, placing the obtained solution A in an evaporator for staged evaporation and crystallization, and obtaining a solid solution mixture of the lithium hydroxide solution according to a set concentration ratio; Step 3, cooling the lithium hydroxide solid solution mixture obtained in step 2 to room temperature, and performing separation operation to obtain a crystalline product B and a filtrate C; Step 4: adding a corresponding proportion of mixed solvent to the crystalline product B obtained in step 3 to perform stirring and washing operations to obtain a solid solution mixture of lithium hydroxide again; Step 5: filtering and separating the lithium hydroxide solid solution mixture obtained in step 4 to obtain a crystalline product D and a filtrate E; Step 6: Use a dissolving agent according to a proportion to perform an elution operation on the crystal product D, and dry it to obtain the desired crystal product; At the same time, during the entire process of preparing battery-grade lithium hydroxide by the dissolution crystallization method, the filtrate E obtained in the process is collected and concentrated again and subjected to dissolution crystallization operations to improve the overall yield of the process; at the same time, the low-boiling point dissolution agent can also be recycled by distillation operations.
2. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that: In step 1, the solvent is an ethanol solution, and its concentration is selected from 75% ethanol solution, 95% ethanol solution and anhydrous ethanol. The mass ratio of the solvent to deionized water is 1: (1-10).
3. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that: The step evaporation crystallization in step 2 refers to the use of different temperatures to perform progressive rotary evaporation crystallization on the solution during the evaporation crystallization process.
4. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that: In step 2, the first stage rotary evaporation temperature is 30-40°C, the time is 5-10min, the rotary evaporation speed is 40-60r / min, the second stage rotary evaporation temperature is 60-75°C, the time is 60-100min, the rotary evaporation speed is 60-100r / min, the absolute pressure of the device is 40-100hPa, and the concentration ratio of the obtained solid solution mixture, in which the mass of solid to liquid is 1:(1.5-2).
5. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that: In step 3, the cooling temperature of the solid solution mixture is 20-30° C., and the stirring speed is 200-500 r / min. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that in step 4, the dissolution agent is selected as an ethanol solution, and its concentration is selected as 75% ethanol solution, 95% ethanol solution and anhydrous ethanol, the mass of the dissolution agent and deionized water is 1: (1-5), the oil bath temperature is 20-30 ° C, the stirring speed is 200-500r / min, and the stirring time is 2-4h.
6. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that: In step 5, the filtration time is 3-5 minutes.
7. A process for purifying battery-grade lithium hydroxide monohydrate by dissolution crystallization according to claim 1, characterized in that: The reagent used for the elution operation in step six is an ethanol solution, the mass ratio of the crystallized product to the elution reagent is (4-6):1, the oven pressure is 10-30Pa, the oven temperature is 70-100°C, the vacuum drying time is 12-24h, and the waste liquid after dissolution and crystallization is recovered by distillation and the ethanol solution is reused.