Amorphous halogen-oxygen compound-containing positive electrode material and preparation method and application thereof

The formation of amorphous halo-oxygen compound positive electrode material through one-step ball milling method solves the problems of high cost of amorphous electrode materials and complex synthesis processes in the prior art, and realizes high-performance and low-cost energy storage materials, which significantly improves circulation Capacity and electrochemical properties.

CN118954616APending Publication Date: 2024-11-15NINGBO EASTERN INSTITUTE FOR ADVANCED STUDY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017830.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing amorphous electrode materials are costly and difficult to achieve efficient and low-cost high-performance energy storage materials in large-scale applications.

Method used

The one-step ball milling method is used to corrode and react solid solution with the crystalline phase positive electrode material to form amorphous halo-oxygen compounds, simplify the synthesis process, reduce production costs, and realize the component gradient distribution of the core-shell structure.

Benefits of technology

It achieves high ion conduction rate and low expansion coefficient, significantly improves the circulation capacity and electrochemical performance of the cathode material, reduces volume changes, simplifies the production process, and lays the foundation for large-scale commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954616A_ABST
    Figure CN118954616A_ABST
Patent Text Reader

Abstract

The invention discloses a positive electrode material containing an amorphous halogen-oxygen compound and a preparation method and application thereof.The preparation method of the positive electrode material containing the amorphous halogen-oxygen compound comprises the steps that a crystalline phase positive electrode material and at least one metal halide are subjected to ball milling treatment, and converting the metal halide into an amorphous halogen-oxygen compound through corrosion and solid solution reaction in the ball milling process, and forming the amorphous halogen-oxygen compound on the surface of the crystalline phase positive electrode material to obtain the positive electrode material containing the amorphous halogen-oxygen compound. The positive electrode material provided by the invention has a relatively high ion transfer rate and a relatively low expansion coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a positive electrode material containing an amorphous halogen-oxygen compound, and a preparation method and application thereof. Background Art

[0002] Alkali metal ion batteries and supercapacitors are considered to be ideal energy storage devices in the next generation of energy storage systems. These energy storage devices are an indispensable part of future green energy. Therefore, it is urgent to develop high-performance, low-cost, and environmentally friendly electrode materials to meet the requirements of high energy density and long cycle life. To date, a variety of crystalline electrodes have been intensively studied, including carbon-based, alloy-based, and organic-based. The strategies to improve the electrochemical performance of these electrodes are summarized as follows: (1) unique structural design to balance morphology and surface area; (2) reducing the size of active materials; (3) doping heteroatoms / introducing vacancies; (4) self-supporting substrates; (5) constructing heterostructures. Although these methods have greatly improved the electrochemical performance of various energy storage systems, the pursuit of low-cost, simple, and scalable electrode materials should continue to be developed.

[0003] Amorphous materials differ from crystals in physical and chemical properties and show great potential as excellent electrode materials. In general, amorphous materials are ordered in a short range at the level of a few atoms, and these ordered regions are randomly connected (long-range disorder). Therefore, amorphous and crystalline materials can be easily distinguished by basic characterization techniques, such as X-ray diffraction: X-rays scatter in many directions, which for amorphous phases will result in a large bump distributed over a wide range, rather than a high-intensity narrow peak (X-rays are scattered only in certain directions); high-resolution transmission electron microscopy: amorphous materials do not show lattice fringes and no diffraction rings, while crystals do the opposite. Due to their unique structure, amorphous materials have significant advantages, such as isotropy and reproducibility. Based on these characteristics, it has been confirmed that amorphous materials have superior energy storage properties compared to crystalline electrodes in energy storage devices.

[0004] In order to improve the energy storage performance of amorphous electrodes, technicians in this field mainly focus on constructing heterostructures (amorphous / crystalline composites and hybridization with carbon), defect engineering (vacancies and heteroatom doping), morphology control (3D structures and 2D ultrathin nanosheets), etc. There is no doubt that the above strategies are effective methods to improve electrochemical performance, but as the cost of their modification continues to increase, large-scale application is difficult to achieve. The development of new amorphous materials with excellent cycle stability and high capacity is necessary, but also a challenge. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a new amorphous positive electrode material and a preparation method thereof. The present invention provides a positive electrode material containing an amorphous halogen-oxygen compound and a preparation method and application thereof to solve the above-mentioned problem. The present invention adopts a one-step ball milling method, abandons complex and tedious synthesis steps, effectively reduces production costs, and the method is highly universal. Finally, a new amorphous material with excellent cycle stability and high capacity is developed, laying a foundation for the large-scale production of the next generation of positive electrode materials containing amorphous halogen-oxygen compounds.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a positive electrode material containing an amorphous halogen-oxygen compound comprises the steps of:

[0008] A crystalline positive electrode material and at least one metal halide MX y After ball milling, the metal halide is converted into an amorphous halogen-oxygen compound through corrosion and solid solution reaction during the ball milling process, and is formed on the surface of the crystalline phase positive electrode material, thereby obtaining a positive electrode material containing an amorphous halogen-oxygen compound;

[0009] Metal Halide MX y wherein M includes at least one metal element other than a radioactive metal element, X includes at least one halogen, and y is an integer between 1 and 6;

[0010] The crystalline phase positive electrode material includes at least one of: lithium ion battery layered material, spinel material, lithium-rich material, olivine material, sodium ion battery transition metal oxide material, polyanion compound material, and Prussian blue compound positive electrode material.

[0011] Metal Halide MX y In the formula, M includes at least one metal element other than radioactive metal elements, X includes at least one halogen, and y is the number of halogen atoms, which is determined according to the valence state of the metal element and is usually an integer between 1 and 6. Metal halide MX y Various compounds formed of these metal elements and the above-mentioned halogen elements may be used.

[0012] The present application provides a positive electrode material containing an amorphous halogen-oxygen compound, and a preparation method and application thereof. The positive electrode material provides defects and vacancies as a lithium / sodium storage positive electrode material. Unlike the disadvantage of traditional amorphous positive electrode materials that cannot deeply deintercalate lithium, the amorphous structure in the amorphous material can alleviate the mechanical strain caused by the insertion and removal of ions, and is less affected by shape rearrangement and volume change, which can ensure the stability of the structure during the deintercalation of lithium. For example, in this application, aluminum chloride, a halide, is used as a dissociator. After the ball milling dissociation reaction with lithium cobalt oxide, a large number of defect sites and Al-O-Cl amorphous amorphous structures are generated on the surface of lithium cobalt oxide, which provides a large number of channels for rapid transmission of lithium ions, significantly enhancing the cycle capacity of the positive electrode material. The existence of such amorphous structures can also be proved by the corresponding XRD and TEM data. At the same time, in practical applications, most of the synthesis processes of amorphous materials are complex and expensive; this work is different from traditional processes such as solid phase method, solution gel method, combustion method, etc., and adopts a simple one-step ball milling synthesis method to achieve rapid and large-scale preparation, laying a solid foundation for its commercial application.

[0013] In the preparation method provided in the present application, corrosion and solid solution reaction refers to the chemical reaction between metal halide and crystalline positive electrode material during ball milling, which can realize the conversion of metal halide into amorphous halogen-oxygen compound and form on the surface interface of crystalline positive electrode material to obtain positive electrode material containing amorphous halogen-oxygen compound. The present application can realize a core-shell structure with a component content gradient distribution, in which the halogen component gradient increases from the inner core to the outer shell and the transition metal element component gradient decreases.

[0014] The positive electrode material prepared by the preparation method of the present application has a high ion transfer rate and a low expansion coefficient, and can achieve both> 10 -7 S / cm High ionic conductivity with >10 -4 S / cm high electron conduction rate, even can achieve>10 -5 S / cm High ionic conductivity with >10 -2 S / cm high electron conduction rate. The cathode material prepared by the preparation method of the present application can achieve an increase of more than 500 times in room temperature ion conduction rate compared with the corresponding crystalline phase cathode material, and reduce the volume change by >30% during the electrochemical cycle.

[0015] Further optionally, when a crystalline phase positive electrode material and a metal halide are used as raw materials, the mass ratio is: 1:1-19.

[0016] Taking into account the actual production cost control, the minimum mass content of the positive electrode material is not less than 50%.

[0017] According to experimental test results, in order to ensure the actual battery application effect after material dissociation, the minimum mass content of halide shall not be less than 5%.

[0018] Further optionally, when a crystalline phase positive electrode material and two metal halides are used as raw materials, the mass ratio is: 1:1:18 to 1:1:2.

[0019] Taking into account the actual production cost control, the minimum mass content of the positive electrode material is not less than 50%.

[0020] According to experimental test results, in order to ensure the actual battery application effect after material dissociation, the minimum mass content of each halide shall not be less than 5%.

[0021] Further optionally, the metal halide includes at least one of aluminum fluoride, aluminum chloride, aluminum bromide, aluminum iodide, lanthanum fluoride, lanthanum chloride, lanthanum bromide, lanthanum iodide, tantalum fluoride, tantalum chloride, tantalum bromide, tantalum iodide, hafnium fluoride, hafnium chloride, hafnium bromide, hafnium iodide, zirconium fluoride, zirconium chloride, zirconium bromide and zirconium iodide.

[0022] Further optionally, the two metal halides include a combination of aluminum chloride and any of the following halides: lanthanum chloride, tantalum chloride, hafnium chloride, zirconium chloride, lanthanum fluoride, lanthanum bromide, lanthanum iodide, tantalum fluoride, tantalum bromide, tantalum iodide, hafnium fluoride, hafnium bromide, hafnium iodide, zirconium fluoride, zirconium bromide and zirconium iodide.

[0023] Further, it may be a combination of aluminum chloride and lanthanum chloride, a combination of aluminum chloride and lanthanum fluoride, a combination of aluminum chloride and lanthanum bromide, a combination of aluminum chloride and lanthanum iodide, a combination of aluminum chloride and tantalum chloride, a combination of aluminum chloride and tantalum fluoride, a combination of aluminum chloride and tantalum bromide, a combination of aluminum chloride and tantalum iodide, a combination of aluminum chloride and hafnium chloride, a combination of aluminum chloride and hafnium fluoride, a combination of aluminum chloride and hafnium bromide, a combination of aluminum chloride and hafnium iodide, a combination of aluminum chloride and zirconium chloride, a combination of aluminum chloride and zirconium fluoride, a combination of aluminum chloride and zirconium bromide, or a combination of aluminum chloride and zirconium iodide.

[0024] Further optionally, the lithium-ion battery layered material includes one of a lithium cobalt oxide material, a ternary NCM material, a high nickel material, a layered lithium-rich manganese-based material, and a layered lithium manganese oxide positive electrode material;

[0025] And / or, the spinel type includes spinel type lithium manganate material;

[0026] And / or, the olivine type material includes lithium iron phosphate material;

[0027] And / or, the sodium ion battery transition metal oxide material comprises a layered material or a tunnel-shaped material;

[0028] And / or, the polyanion compound material includes sodium vanadium phosphate or sodium iron phosphate material.

[0029] Furthermore, the phase positive electrode material includes LiCoO2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiFePO4, LiCoPO4 and Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 At least one of O2.

[0030] Further optionally, during the ball milling treatment, the ball milling speed is 100 rpm to 700 rpm, and the ball milling time is 0.1 h to 48 h.

[0031] A positive electrode material containing an amorphous halogen-oxygen compound comprises an inner core and a shell layer coated outside the inner core; the inner core comprises a crystalline phase positive electrode material; the outer shell comprises an amorphous halogen-oxygen compound; the crystalline phase positive electrode material comprises at least one of a lithium ion battery layered material, a spinel material, a lithium-rich material, an olivine material, a sodium ion battery transition metal oxide material, a polyanion compound material, and a Prussian blue compound positive electrode material; the amorphous halogen-oxygen compound is an amorphous halogen-oxygen metal compound, wherein the metal element contained therein comprises at least one of metal elements other than radioactive metal elements.

[0032] The positive electrode material containing amorphous halogen-oxygen compound provided in the present application is a core-shell structure, wherein the core comprises a crystalline positive electrode material, and the surface shell comprises an amorphous halogen-oxygen compound material, which has a high ion transfer rate and a low expansion coefficient, and can achieve both>10 -7 S / cm High ionic conductivity with >10 -4 S / cm high electron conduction rate, even can achieve>10 -5 S / cm High ionic conductivity with >10 -2 S / cm high electron conduction rate.

[0033] The amorphous halogen-oxygen metal compound, wherein the metal element contained therein includes at least one of the metal elements other than the radioactive metal element. Further, the metal elements other than the radioactive metal element (such as polonium, radon, francium, radium, actinium, thorium, protactinium, uranium, neptunium, plutonium) include but are not limited to lithium, sodium, potassium, magnesium, calcium, aluminum, lanthanum, tantalum, hafnium, zirconium, etc.

[0034] Further optionally, the metal element contained in the amorphous halogen-oxygen metal compound includes at least one of aluminum, lanthanum, tantalum, hafnium and zirconium.

[0035] Further optionally, from the inner core to the outer shell, the halogen content increases in gradient, and the metal element content decreases in gradient. The "transition metal" herein refers to the transition metal element in the crystalline phase positive electrode material.

[0036] Further optionally, the positive electrode material containing the amorphous halogen-oxygen compound is prepared by the above-mentioned preparation method.

[0037] A positive electrode plate comprises the positive electrode material containing the amorphous halogen-oxygen compound or the positive electrode material prepared by the above-mentioned preparation method.

[0038] A battery comprises the above-mentioned positive electrode plate.

[0039] The present invention has the following advantages and beneficial effects:

[0040] 1. In the preparation process of the present invention, the halide and the positive electrode material are directly ball-milled by a simple ball-milling method. The operation steps are simple, the raw material source is simple and easy to prepare, and no complicated synthesis conditions are required, which significantly improves production efficiency and saves preparation costs.

[0041] 2. The present invention provides a positive electrode material containing an amorphous halogen-oxygen compound with defects and vacancies as a lithium / sodium storage positive electrode material. The positive electrode material has multiple alkali metal ion storage sites and diffusion channels, and the volume change during the cycle is alleviated. It has a higher ion transfer rate and a lower expansion coefficient, and has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0043] Figure 1 This is the TEM lattice image of the positive electrode material containing amorphous halogen-oxygen compounds provided in Example 1.

[0044] Figure 2 This is a TEM morphology image of the positive electrode material containing amorphous halogen-oxygen compounds prepared in Example 1.

[0045] Figure 3 This is the SEM morphology of the positive electrode material prepared in Comparative Example 3.

[0046] Figure 4 This is the SEM morphology of the positive electrode material prepared in Comparative Example 4.

[0047] Figure 5 1 is the XRD pattern of the positive electrode material containing amorphous halogen-oxygen compounds prepared in Example 1.

[0048] Figure 6 This is the charge and discharge curve of the positive electrode material containing amorphous halogen-oxygen compound prepared in Example 1 at 0.5C.

[0049] Figure 7This is the cycle curve of the positive electrode material containing amorphous halogen-oxygen compound prepared in Example 1 at 0.5C.

[0050] Figure 8 This is the cycle curve of the positive electrode material prepared in Comparative Example 3 at 0.5C.

[0051] Fig. 9 This is the cycle curve of the positive electrode material prepared in Comparative Example 4 at 0.5C. DETAILED DESCRIPTION

[0052] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0053] Example 1

[0054] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0055] Step 1: Add 0.4 g aluminum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0056] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 1:4.

[0057] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0058] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0059] Comparative Example 1

[0060] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0061] Step 1: Add 0.4 g aluminum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0062] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 1:4.

[0063] Step 2: After each 10 minutes of ball milling, pause for 5 minutes and then continue ball milling; then repeat the above steps, the total ball milling time is controlled to be 50 hours, and the ball milling speed is maintained at 500 rpm.

[0064] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0065] Comparative Example 2

[0066] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0067] Step 1: Add 0.4 g aluminum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0068] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 1:4.

[0069] Step 2: After each ball milling for 5 min, the ball milling speed was maintained at 500 rpm.

[0070] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0071] Comparative Example 3

[0072] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0073] Step 1: Add 10 g aluminum chloride and 1 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0074] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 10:1.

[0075] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0076] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0077] Comparative Example 4

[0078] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0079] Step 1: Add 0.1 g aluminum chloride and 3.0 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0080] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 1:30.

[0081] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0082] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0083] Example 2

[0084] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0085] Step 1: Add 0.4 g tantalum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0086] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 1:4.

[0087] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0088] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0089] Example 3

[0090] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0091] Step 1: Add 0.4 g zirconium chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0092] Among them, the mass ratio of aluminum chloride to lithium cobalt oxide is 1:4.

[0093] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0094] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0095] Example 4

[0096] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0097] Step 1: Add 0.4 g zirconium chloride and 1.6 g lithium manganate Li2MnO3 solid powder into a 500 mL high energy ball mill;

[0098] Among them, the mass ratio of aluminum chloride to lithium manganese oxide Li2MnO3 is 1:4.

[0099] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0100] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0101] Example 5

[0102] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0103] Step 1: Add 0.4 g zirconium chloride and 1.6 g lithium iron phosphate LiFePO4 solid powder into a 500 mL high energy ball mill;

[0104] Among them, the mass ratio of aluminum chloride to lithium iron phosphate LiFePO4 is 1:4.

[0105] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0106] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0107] Example 6

[0108] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0109] Step 1: Add 0.4 g aluminum chloride and 1.6 g sodium vanadium phosphate solid powder into a 500 mL high energy ball mill;

[0110] Wherein, the mass ratio of aluminum chloride to sodium vanadium phosphate is 1:4.

[0111] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0112] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0113] Example 7

[0114] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0115] Step 1: Add 0.4 g aluminum chloride and 1.6 g sodium iron phosphate solid powder into a 500 mL high energy ball mill;

[0116] Among them, the mass ratio of aluminum chloride to sodium iron phosphate is 1:4.

[0117] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0118] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0119] Example 8

[0120] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0121] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0122] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium cobalt oxide is 1:1:8.

[0123] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0124] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0125] Comparative Example 5

[0126] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0127] Step 1: Add 0.67 g aluminum chloride, 0.67 g lanthanum chloride and 0.67 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0128] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium cobalt oxide is 1:1:1.

[0129] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0130] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0131] Comparative Example 6

[0132] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0133] Step 1: Add 0.095 g aluminum chloride, 0.095 g lanthanum chloride and 1.80 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0134] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium cobalt oxide is 1:1:19.

[0135] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0136] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0137] Example 9

[0138] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0139] Step 1: Add 0.1 g aluminum chloride, 0.1 g lanthanum chloride and 1.8 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0140] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium cobalt oxide is 1:1:18.

[0141] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0142] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0143] Example 10

[0144] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0145] Step 1: Add 0.2 g aluminum chloride, 0.2 g zirconium chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0146] Among them, the mass ratio of aluminum chloride, zirconium chloride and lithium cobalt oxide is 1:1:8.

[0147] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0148] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0149] Comparative Example 7

[0150] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0151] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0152] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium cobalt oxide is 1:1:8.

[0153] Step 2: After each ball milling for 4 min, the ball milling speed was maintained at 500 rpm.

[0154] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0155] Comparative Example 8

[0156] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0157] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0158] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium cobalt oxide is 1:1:8.

[0159] Step 2: After each 10 minutes of ball milling, pause for 5 minutes and then continue ball milling; then repeat the above steps, the total ball milling time is controlled to be 60 hours, and the ball milling speed is maintained at 500 rpm.

[0160] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0161] Embodiment 11

[0162] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0163] Step 1: Add 0.2 g aluminum chloride, 0.2 g zirconium chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0164] Among them, the mass ratio of aluminum chloride, zirconium chloride and lithium cobalt oxide is 1:1:8.

[0165] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0166] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0167] Example 12

[0168] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0169] Step 1: Add 0.2 g aluminum chloride, 0.2 g hafnium chloride and 1.6 g lithium cobalt oxide solid powder into a 500 mL high energy ball mill;

[0170] Among them, the mass ratio of aluminum chloride, hafnium chloride and lithium cobalt oxide is 1:1:8.

[0171] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0172] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0173] Example 13

[0174] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0175] Step 1: Add 0.2g aluminum chloride, 0.2g tantalum chloride and 1.6g NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2) solid powder;

[0176] Among them, aluminum chloride, tantalum chloride and NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2) has a mass ratio of 1:1:8.

[0177] Step 2: Ball milling for 10 min, with the ball milling speed maintained at 500 rpm.

[0178] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0179] Embodiment 14

[0180] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0181] Step 1: Add 0.1 g aluminum chloride, 0.1 g lanthanum chloride and 1.8 g lithium iron phosphate LiFePO4 solid powder into a 500 mL high energy ball mill;

[0182] Among them, the mass ratio of aluminum chloride, lanthanum chloride and lithium iron phosphate LiFePO4 is 1:1:18.

[0183] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0184] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0185] Embodiment 15

[0186] This embodiment provides a positive electrode material containing an amorphous halogen-oxygen compound, and the specific preparation method is as follows:

[0187] Step 1: Add 0.1 g aluminum chloride, 0.1 g lanthanum chloride and 1.8 g sodium iron phosphate solid powder into a 500 mL high energy ball mill;

[0188] Among them, the mass ratio of aluminum chloride, lanthanum chloride and sodium iron phosphate is 1:1:18.

[0189] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0190] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0191] 1. Electron microscopy analysis:

[0192] Figure 1 is a TEM lattice image of the positive electrode material containing amorphous halogen-oxygen compound provided in Example 1. Figure 1 It can be seen from the TEM image that the material after ball milling of lithium cobalt oxide and aluminum chloride has obvious amorphous regions. In addition, the obvious lattice region in the figure is residual lithium cobalt oxide.

[0193] Figure 2 This is a TEM morphology of the positive electrode material containing amorphous halogen-oxygen compound prepared in Example 1. It can be observed that the structure of lithium cobalt oxide and aluminum chloride remains intact after ball milling without obvious damage.

[0194] Figure 3 This is a SEM image of the positive electrode material prepared in Comparative Example 3. It can be observed that when the mass ratio of aluminum chloride ball milling is too high, most of the solid solution positive electrode particles are halides, and no obvious positive electrode particles appear, indicating that the solid solution positive electrode is not successfully prepared.

[0195] Figure 4 This is a SEM image of the positive electrode material prepared in Comparative Example 4. It can be observed that when the mass ratio of lithium cobalt oxide ball milling is too high, most of the solid solution positive electrode particles are in the shape of lithium cobalt oxide particles themselves, and only a small amount of positive electrode particles are dissociated from aluminum chloride, and an ideal product cannot be obtained.

[0196] 2. X-ray diffraction analysis:

[0197] Figure 5 1 is the XRD pattern of the positive electrode material containing amorphous halogen-oxygen compounds prepared in Example 1. Figure 5 It can be clearly seen that the sharp peak of lithium cobalt oxide at around 20° disappears and becomes a broad diffraction peak, further proving that the material after ball milling generates an amorphous phase.

[0198] 2. Performance Test

[0199] 1. Preparation of batteries:

[0200] The all-solid-state battery positive electrode active material and LiIn negative electrode using the prepared amorphous positive electrode combination were assembled in an argon-filled glove box. First, about 120 mg of Li6PS5Cl powder was pressed at 100 MPa for 1 min (diameter 10 mm). A composite positive electrode mixture was prepared by mixing the positive electrode active material, Li6PS5Cl and carbon black in a weight ratio of 70:30:1. On the Li6PS5Cl side of the solid electrolyte particle, about 10 mg of the composite positive electrode mixture was spread and pressed at 300 MPa for 2 minutes. On the other side of the particle, a thin indium foil (diameter 10 mm) was attached, and about 2 mg of lithium foil was pressed into a thin layer and placed on the indium foil. The mass loading of the composite positive electrode is 8 mg cm -2 .

[0201] 2. Test method:

[0202] The constant current charge / discharge voltage was set to 2.5V-4.3V relative to Li+ / Li. The charge and discharge curve test was performed at a current density of 0.1c. The cycle performance test was performed at a current density of 0.5c.

[0203] 3. Test results:

[0204] like Figure 6 and Figure 7 As shown, the capacity of the positive electrode material provided in Example 1 remained stable at 110 mAh g after 50 cycles at 0.5 c. -1 In the first cycle at a current density of 0.1c, the discharge capacity can reach 130mAh g -1 , the first-cycle Coulomb efficiency is 94.8%.

[0205] like Figure 8 and Fig. 9 As shown in the figure, the positive electrode materials provided in Comparative Examples 3 and 4 exhibited completely different electrochemical performances after 50 cycles at 0.5C. The positive electrode prepared in Comparative Example 3 had a first cycle capacity of only 70 mAh g -1 After 50 cycles, the battery decayed to 25 mAh g -1 The positive electrode prepared in Comparative Example 4 has a more stable cycle performance than that in Comparative Example 3, but its capacity is still seriously attenuated compared with that in Example 1. After 50 cycles, the capacity is only 75 mAh g -1 .

[0206] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a positive electrode material containing an amorphous halogen-oxygen compound, characterized in that: Includes steps: A crystalline positive electrode material and at least one metal halide MX y After ball milling, the metal halide is converted into an amorphous halogen-oxygen compound through corrosion and solid solution reaction during the ball milling process, and is formed on the surface of the crystalline phase positive electrode material, thereby obtaining a positive electrode material containing an amorphous halogen-oxygen compound; The metal halide MX y wherein M includes at least one metal element other than a radioactive metal element, X includes at least one halogen, and y is an integer between 1 and 6; The crystalline phase positive electrode material includes at least one of: lithium ion battery layered material, spinel material, lithium-rich material, olivine material, sodium ion battery transition metal oxide material, polyanion compound material, and Prussian blue compound positive electrode material.

2. The method for preparing a positive electrode material containing an amorphous halogen-oxygen compound according to claim 1, characterized in that: When the crystalline phase positive electrode material and a metal halide are used as raw materials, the mass ratio is: 1:1-19; Alternatively, when a crystalline positive electrode material and two metal halides are used as raw materials, the mass ratio is 1:1:18 to 1:1:

2.

3. The method for preparing a positive electrode material containing an amorphous halogen-oxygen compound according to claim 1, characterized in that: The metal halide includes at least one of aluminum fluoride, aluminum chloride, aluminum bromide, aluminum iodide, lanthanum fluoride, lanthanum chloride, lanthanum bromide, lanthanum iodide, tantalum fluoride, tantalum chloride, tantalum bromide, tantalum iodide, hafnium fluoride, hafnium chloride, hafnium bromide, hafnium iodide, zirconium fluoride, zirconium chloride, zirconium bromide and zirconium iodide.

4. The method for preparing a positive electrode material containing an amorphous halogen-oxygen compound according to claim 1, characterized in that: During the ball milling treatment, the ball milling speed is 100 rpm to 700 rpm, and the ball milling time is 0.1 h to 48 h.

5. A positive electrode material containing an amorphous halogen-oxygen compound, characterized in that: It comprises an inner core and a shell layer covering the outer core; The inner core includes a crystalline positive electrode material; The shell includes an amorphous halogen-oxygen compound; The crystalline phase positive electrode material includes at least one of a lithium ion battery layered material, a spinel material, a lithium-rich material, an olivine material, a sodium ion battery transition metal oxide material, a polyanion compound material, and a Prussian blue compound positive electrode material; The amorphous halogen-oxygen compound is an amorphous halogen-oxygen metal compound, wherein the metal element contained therein includes at least one of metal elements other than radioactive metal elements.

6. The positive electrode material containing an amorphous halogen-oxygen compound according to claim 5, characterized in that: The metal element contained in the amorphous halogen-oxygen metal compound includes at least one of aluminum, lanthanum, tantalum, hafnium and zirconium.

7. The positive electrode material containing an amorphous halogen-oxygen compound according to claim 5, characterized in that: From the inner core to the outer shell, the halogen content increases gradually, and the transition metal element content decreases gradually.

8. The positive electrode material containing an amorphous halogen-oxygen compound according to any one of claims 5 to 7, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 4.

9. A positive electrode sheet, characterized in that: A positive electrode material comprising the amorphous halogen-oxygen compound according to any one of claims 1 to 4, or a positive electrode material prepared by the preparation method according to any one of claims 5 to 8.

10. A battery, characterized in that: Including the positive electrode sheet as described in claim 9.