Method for directly preparing cast stone pipe by utilizing molten metallurgical slag

Through high-temperature melted metallurgical slag and centrifugal casting technology, the problems of low utilization rate of metallurgical slag and poor performance of microcrystalline cast stone pipes are solved, and efficient and low-cost production of wear-resistant and corrosion-resistant cast stone pipes are achieved.

CN118954982APending Publication Date: 2024-11-15JIANGSU YUANSHI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410923567.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the utilization rate of metallurgical slag is low, resulting in high energy consumption and high production costs. The processing of microcrystal cast stone pipes is complex and has poor performance, making it difficult to meet the needs of wear resistance and corrosion resistance.

Method used

High-temperature molten metallurgical slag is used as raw material, and by adjusting the melt viscosity and homogenization treatment, combined with centrifugal casting method, wear-resistant and corrosion-resistant casting pipes are prepared to reduce energy consumption and improve the utilization rate of metallurgical slag.

Benefits of technology

It realizes efficient utilization of metallurgical slag, reduces energy consumption and production costs, improves the wear and corrosion resistance of cast stone pipes, and has a simple process and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954982A_ABST
    Figure CN118954982A_ABST
Patent Text Reader

Abstract

The invention relates to a method for directly preparing a cast stone pipe by using molten metallurgical slag. The method comprises the following steps: 1, adjusting and homogenizing melt viscosity; 2, pretreating a casting mold; 3, casting and molding; and 3, casting and molding, wherein the temperature of the melt is controlled within the range of 1100-1300 DEG C, and the viscosity of the high-temperature melt is controlled within the range of 0.5-15 Pa.s. 4, pipe blank heat treatment; and 5, pipeline finish machining. According to the method, molten metallurgical slag and industrial waste residues or chemical reagents are used as a tempering agent to improve the melt viscosity, a centrifugal casting mode is adopted for casting forming, and then nucleation, crystallization and finish machining are conducted to obtain the finished cast stone pipe. In the preparation process of the cast stone pipe, the utilization rate of single metallurgical slag exceeds 70%, the production process is energy-saving and environment-friendly, the production cost is low, and the application is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of microcrystalline cast stone pipes, and in particular to a method for directly preparing wear-resistant and corrosion-resistant cast stone pipes by utilizing molten metallurgical slag. Background Art

[0002] Metallurgical slag is a by-product of the smelting process. Unused metallurgical slag is piled up in large quantities, and most of it is piled up in the open air, which not only occupies land, but also easily causes dust pollution, mudslides, river siltation and other hazards. Harmful leachates in the waste slag are easy to pollute water bodies and harm the environment. The main components of metallurgical slag are generally SiO 2 、CaO、Al 2 O 3 , MgO and other oxides, which are also important raw materials required for industrial production.

[0003] As a device for conveying fluid substances, pipelines are widely used in chemical, petroleum, metallurgy, power generation and other industries. Therefore, there is a great market demand for wear-resistant, corrosion-resistant and low-cost pipes. Most pipes on the market have poor comprehensive performance. For example, steel pipes are prone to corrosion in humid or corrosive environments, resulting in pipeline failure and high self-weight and maintenance costs; plastic pipes are usually extremely sensitive to operating temperature, have poor pressure resistance, and have poor corrosion resistance to certain chemicals.

[0004] Microcrystalline cast stone pipe is a high-performance wear-resistant and corrosion-resistant pipe material. It is a new type of silicate crystal material. Its main raw materials include blast furnace slag, diabase, basalt, etc., and silica sand and an appropriate amount of crystal nucleating agent are added. This pipe material has excellent wear resistance, corrosion resistance, compression resistance, flexural resistance, impact resistance and temperature difference resistance, and can be used in cement industry, steel industry, coking industry and other fields.

[0005] In the prior art, patent applications / patents for microcrystalline cast stone pipes can be roughly divided into two categories: one category is mostly composite pipes, and the other category has a low utilization rate of single industrial waste residues. For example:

[0006] China's invention patent application publication number CN108975713A discloses a 'method for preparing a pipe composited with wear-resistant microcrystalline glass'. The technical solution is to fix the microcrystalline glass tube to the metal pipe by an adhesive after the metal pipe and microcrystalline glass tube are made to form a composite wear-resistant microcrystalline glass pipe. Although composite pipes have the characteristics of high hardness, high toughness and light weight, their processing and manufacturing are complex. Under high pressure or frequent pressure changes, different material layers of the composite pipe may be delaminated and separated, affecting the performance of the pipe.

[0007] China Invention Patent Application Publication No. CN102173588B discloses a 'slag microcrystalline glass tube and its preparation method'. The raw materials of this technical solution are fly ash, industrial waste slag (slag after re-selection of Bayan Obo tailings, blast furnace slag, steel slag, etc.) and quartz sand, which are added to a ball mill mixer and mixed evenly to prepare a mixture; the mixture is added to a glass melting furnace and melted at 1350-1450°C; the molten melt is poured into a centrifugal pipe casting machine to prepare microcrystalline glass tubes by centrifugal casting. The wear resistance of the microcrystalline glass tube is improved compared with that of the cast stone tube, but its formula is complex and requires the addition of a variety of industrial waste slags and conditioning agents, and the utilization rate of a single industrial waste slag is low. Summary of the invention

[0008] The purpose of the present invention is to improve the deficiencies of the above-mentioned prior art and obtain a method for producing cast stone pipes by directly using high-temperature molten metallurgical slag as raw material, which can make full use of waste heat, reduce energy consumption, and further adapt to industrial production.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] A method for directly producing a cast stone pipe using molten metallurgical slag, wherein: the method comprises the following steps:

[0011] (1) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into a heat-insulating slag ladle, and a conditioning agent is added to adjust the melt viscosity. The raw material composition in the heat-insulating slag ladle is as follows: 5-30% conditioning agent and the rest is molten metallurgical slag; then, the slag is kept at 1430-1555°C for 30-120 minutes. During the heat-insulating period, the scum and bubbles of the melt are removed by stirring or adding a clarifier, so that the melt is fully clarified and the whole is homogenized;

[0012] (2) Casting mold pretreatment: Before casting, a coating such as resin sand or a mold release agent is applied to the inside of the centrifugal casting machine pipe mold; then, a metal support structure is made into a cylindrical shape suitable for the mold, the diameter of the support structure is slightly smaller than the inner diameter of the mold and is placed in the mold, and fixed at a position 1 to 30 mm away from the inner surface of the centrifugal casting machine mold through a preset positioning structure inside the mold;

[0013] (3) Casting: The melt temperature is controlled within the range of 1100 to 1300°C, and the high temperature melt viscosity is controlled within the range of 0.5 to 15 Pa·s; the melt is poured into a preheated mold by mobile casting, and centrifugally cast at a speed of 500 to 2000 rpm to obtain a tube blank;

[0014] (4) Heat treatment of the tube blank: After the tube blank is cooled to the demoulding temperature, a demoulding device is used to separate the tube blank from the mold. The demoulding tube blank is moved to a tunnel kiln and subjected to nucleation and crystallization treatment at 600 to 1000° C. for 0.5 to 6 hours. The crystallized tube blank is then cooled at a uniform rate or cooled in the furnace to obtain a cast stone tube.

[0015] (5) Pipe finishing: The surface and inner wall of the cast stone pipe are cleaned, polished and ground to obtain the final product.

[0016] In the step (1), the conditioning agent is divided into coal gangue, high-boron raw materials or other industrial waste residues and chemical reagents, wherein the high-boron raw materials are one or more mixtures of borax and high-boron tailings, the industrial waste residues are coal gangue, rock wool fibers, etc., the chemical reagents are calcium fluoride, boron oxide, etc.; the clarifier is one or more mixtures of industrial-grade antimony oxide and industrial-grade sodium chloride.

[0017] The molten metallurgical slag is selected from metallurgical waste slags such as nickel-iron slag, chromium-iron slag, vanadium-titanium blast furnace slag, etc. The molten slag is used at a temperature of 1500-1600° C. The clarifier accounts for 0-2% of the mass of the added conditioning agent.

[0018] In the step (3), the release agent is one of dry coatings selected from silica powder, diatomaceous earth or corundum powder; or a water-based coating made from the dry coating according to a certain ratio.

[0019] In the step (3), the pouring method is mobile pouring, and the pouring port is radially fed into the pipe mold at a uniform speed, wherein the direction in which the melt flows in should be tangent to the direction of rotation of the mold;

[0020] The centrifugal casting machine is a horizontal centrifuge, the temperature range during centrifugal casting is 1100-1300°C, the rotation speed of the horizontal centrifuge is 500-2000 rpm, and the angle of centrifugal casting is 0-10°.

[0021] In the step (3), the melt viscosity of the high-temperature melt is controlled within the range of 0.5 to 5 Pa·s at 1200 to 1300° C.; and the melt viscosity is controlled within the range of 4 to 15 Pa·s at 1100 to 1200° C.

[0022] In the step (4), in the demolding treatment, the demolding temperature is 700-800°C; in the nucleation treatment, the nucleation temperature is 600-800°C, and the holding time is 0.5-3h; in the crystallization treatment, the crystallization temperature is 800-1000°C, and the holding time is 0.5-3h, and then the temperature is uniformly reduced at a rate of 2-10°C / min, or it is directly taken out when it is cooled to below 200°C in the furnace.

[0023] The conditioning agent is selected from SiO 2 、CaO、Al2 O 3 , rock wool fiber, B 2 O 3 , CaF 2 , rock wool fiber, borax pentahydrate, CaF 2 At least one of .

[0024] In the step (1), the preset positioning structure inside the mold is a groove or a bracket.

[0025] The chemical composition of the cast stone pipe in the use state is as follows: MgO: 15% to 40%, Fe 2 O 3 : 1% to 10%, FeO: 1% to 5%, Al 2 O 3 : 2% ~ 8%, CaO: 8% ~ 25%, Cr 2 O 3 :0.1%~5%,Na 2 O and K 2 O: 0.1% to 3%, the rest is SiO 2 .

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention directly uses molten metallurgical slag to add a tempering agent to adjust the viscosity, which fully utilizes the sensible heat of the molten slag. Compared with the prior art of mixing a variety of industrial waste slags and then melting them for casting, the present invention saves energy and is more in line with the concept of low carbon and environmental protection.

[0028] Aiming at the shortcomings of existing microcrystalline cast stone pipes, the present invention optimizes the formula ingredients, adjusts the casting heat treatment system, and invents a method for efficiently utilizing a single metallurgical slag to cast wear-resistant and corrosion-resistant cast stone pipes. Among them:

[0029] 1. As solid waste, metallurgical slag has a high utilization rate, which effectively realizes the effective utilization of waste resources and proposes a new way out for the resource recycling of metallurgical slag;

[0030] 2. The formula of cast stone pipe is simple, with only metallurgical slag and a small amount of conditioning agent. The utilization rate of single metallurgical slag is high, and the large-scale production cost is low;

[0031] 3. The present invention adopts a centrifugal casting molding method. Centrifugal casting can wash out impurities in the melt on the surface of the finished product, reduce internal defects, and reduce internal bubbles through centrifugal rotation to make the finished product structure more compact and the finished product has high precision;

[0032] 4. The performance of finished cast stone pipes is higher than the requirements of cast stone construction industry standards. They have good hardness, compressive strength, wear resistance, acid and alkali resistance, and other properties, and have strong market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The XRD phase diagram of the cast stone pipe obtained by the present invention is shown, showing that the main phase of the cast stone pipe is diopside;

[0035] Figure 2-1 to Figure 2-5 The figure shows the longitudinal section diagram of the melt distribution change during the casting process. Figure 2-1 to Figure 2-5 It is a schematic diagram of the longitudinal section of the melt at 0, 10, 30, 50, and 70 seconds of casting. Figure 2-6 Different colors in the graph represent different melt volume fractions in the mold during the casting process;

[0036] Figure 3-1 to Figure 3-5 The figure shows the schematic diagram of melt temperature change during casting; Figure 3-1 to Figure 3-5 This is a schematic diagram of the melt temperature at 0, 2, 6, 10, and 70 seconds of casting. It can be seen that at 10 seconds of casting ( Figure 3-4 ) The temperature is basically stable, Figure 3-6 The different colors in the graph represent different melt temperatures in the mold during the casting process;

[0037] Figure 4 The figure shows a finished product schematic diagram of a cast stone pipe obtained by the present invention;

[0038] Figure 5 It is a schematic structural diagram of the internal hollow columnar wire mesh used in preparing the cast stone pipe by the method of the present invention. DETAILED DESCRIPTION

[0039] The present invention provides a method for directly preparing a cast stone pipe by using molten metallurgical slag, comprising the following steps:

[0040] 1. Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into the insulation slag bag, and a conditioning agent is added to adjust the melt viscosity. The melt is kept at a process temperature of 1430-1555°C. During the insulation period, stirring is used, or a clarifier is added to remove the scum and bubbles in the melt, so that the melt is fully clarified and homogenized as a whole.

[0041] 2. Pretreatment of casting mold: Before casting, line the inside of the centrifugal casting machine pipe mold with resin sand or release agent and other coatings; fix the metal support structure at a distance of 1 to 30 mm from the inner surface of the centrifugal casting machine mold;

[0042] 3. Casting: Control the melt temperature within the range of 1100-1300°C, and the high-temperature melt viscosity within the range of 0.3-10Pa·s; pour into a preheated mold by mobile casting, and centrifugally cast at a certain speed to obtain a tube blank;

[0043] 4. Heat treatment of tube blank: After the tube blank is cooled to the demoulding temperature, a demoulder is used to separate the tube blank from the mold, and the demoulding tube blank is moved to a tunnel kiln for nucleation and crystallization treatment. In the nucleation treatment, the nucleation temperature is 600-800°C, and the holding time is 0.5-3h; in the crystallization treatment, the crystallization temperature is 800-1000°C, and the holding time is 0.5-3h; then the crystallized tube blank is cooled at a uniform speed or cooled with the furnace to obtain a cast stone tube;

[0044] 5. Pipeline finishing: The surface and inner wall of the cast stone pipe are cleaned, polished and ground to obtain the final product.

[0045] In terms of mass percentage, the ratio of the metallurgical slag to the tempering agent is 70:30 to 95:5.

[0046] The microcrystalline cast stone pipe of the present invention is formed by centrifugal casting. Centrifugal casting is a special casting method. In this method, molten material is injected into a rotating mold, and the molten material is evenly distributed inside the mold to shape it with the help of centrifugal force, and impurities are separated to make the structure of the cast product denser.

[0047] When hollow castings are centrifugally cast, and the rotating axis is at an angle with the horizontal plane, the inner surface of the casting after solidification will form a parabolic shape. Small inclination angles are more favorable for melt flow during horizontal centrifugal casting. When the length of the annular casting is more than twice its inner diameter, horizontal centrifugal casting should be considered. Therefore, the present invention gives priority to horizontal centrifugal casting. When manufacturing pipes that are not too long, the mold can be kept at a certain inclination angle with the horizontal ground to ensure that the high-temperature melt flows fully inside the pipe mold.

[0048] The present invention conducts in-depth research on the tempering of high-viscosity molten metallurgical slag (such as nickel-iron slag, etc.). After the high-viscosity metallurgical slag is tempered, the viscosity in a certain temperature range (1100°C to 1550°C) is significantly reduced, which is convenient for molding during the casting process.

[0049] The present invention provides a method for directly preparing a cast stone pipe by utilizing molten metallurgical slag, directly utilizing the molten metallurgical slag, thereby avoiding waste of energy resources. Meanwhile, the process of the present invention does not use raw materials with excessively high costs, thereby minimizing the cost. The produced microcrystalline cast stone pipe is of high quality and has strong market competitiveness.

[0050] The present invention is described in detail below in conjunction with specific embodiments.

[0051] Example 1

[0052] 1) Raw material ratio: by mass percentage, 70% nickel iron slag, 10% SiO 2 , 16% CaO,

[0053] 4%Al 2 O 3 ;

[0054] 2) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into the insulation slag bag and SiO 2 , CaO, Al 2 O 3 Adjust the melt viscosity and keep the melt at a process temperature of 1500°C. During the holding period, remove the scum and bubbles in the melt to make the melt fully clarified and homogenized.

[0055] 3) Casting mold pretreatment: Before casting, quartz sand is lined inside the centrifugal casting machine pipe mold as a coating; then a hollow cylindrical wire mesh with a diameter slightly smaller than the inner diameter of the mold is placed in the mold and fixed at a position 15 mm away from the inner surface of the centrifugal casting machine mold through a preset groove inside the mold;

[0056] 4) Casting: The melt temperature is controlled at 1300°C, at which time the high-temperature melt viscosity is approximately 4 Pa·s; the melt is poured into a preheated mold at a mold speed of 850 r / min to obtain a tube blank;

[0057] 5) Heat treatment of tube blank: After the tube blank is cooled to 800°C, it is demoulded and moved to a tunnel kiln for nucleation and crystallization treatment. The nucleation temperature is 750°C and the holding time is 1.5 hours; in the crystallization treatment, the crystallization temperature is 880°C and the holding time is 1 hour; then the crystallized tube blank is cooled at a speed of 5°C / min to obtain a cast stone tube;

[0058] 6) Pipe finishing: The surface and inner wall of the cast stone pipe are cleaned, polished and ground to obtain the final product.

[0059] 7) The main chemical components of the cast stone pipe are: SiO 2 :44.36%, MgO: 9.42%, Fe 2 O 3 : 5.08%,Al 2 O 3 :13.15%, CaO: 9.67%, Cr 2 O 3 : 0.04%;

[0060] 8) The main physical properties of the cast stone pipe are: Mohs hardness 9, alkali resistance (20% NaOH solution) 99.2%, acid resistance (98% H 2 SO 4 )99.6%, water absorption rate 0.026%, flexural strength 120Mpa, compressive strength 1190Mpa.

[0061] Example 2

[0062] 1) Raw material ratio: by mass percentage, 70.4% nickel iron slag, 17.6% rock wool fiber, 7% B 2 O 3 , 5% CaF 2 ;

[0063] 2) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into the insulation slag bag, and rock wool fiber, B 2 O 3 and CaF 2 Adjust the melt viscosity and keep the melt at a process temperature of 1450°C. During the holding period, remove the scum and bubbles in the melt to make the melt fully clarified and homogenized.

[0064] 3) Casting mold pretreatment: Before casting, quartz sand is lined inside the centrifugal casting machine pipe mold as a coating; then a hollow cylindrical wire mesh with a diameter slightly smaller than the inner diameter of the mold is placed in the mold and fixed at a position 20 mm away from the inner surface of the centrifugal casting machine mold through a preset groove inside the mold;

[0065] 4) Casting: The melt temperature is controlled at 1250°C, at which the high-temperature melt viscosity is approximately 2.7 Pa·s; the melt is poured into a preheated mold at a mold speed of 800 r / min to obtain a tube blank;

[0066] 5) Heat treatment of tube blank: After the tube blank is cooled to 780℃, it is demoulded and moved to a tunnel kiln for nucleation and crystallization treatment. The nucleation temperature is 780℃ and the holding time is 2h; in the crystallization treatment, the crystallization temperature is 900℃ and the holding time is 1.5h; then the tube blank after crystallization treatment is cooled in the furnace to obtain a cast stone tube;

[0067] 6) Pipe finishing: The surface and inner wall of the cast stone pipe are cleaned, polished and ground to obtain the final product.

[0068] 7) The main chemical components of the obtained cast stone pipe are: SiO2: 48.46%, MgO: 25.10%, Fe2O3: 6.98%, Al2O3: 4.06%, CaO: 2.44%, Cr2O3: 1.07%, Na2O1.99%;

[0069] 8) The main physical properties of the cast stone pipe are: Mohs hardness 9, alkali resistance (20% NaOH solution) 98.7%, acid resistance (98% H 2 SO 4 )99.3%, water absorption rate 0.036%, flexural strength 123Mpa, compressive strength 1200Mpa.

[0070] Example 3

[0071] 1) Raw material ratio: by mass percentage, 72% nickel iron slag, 13% rock wool fiber, 12.5% ​​borax pentahydrate (Na 2 B 4 O 7 ·5H 2 O), 2.5% CaF 2 ;

[0072] 2) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into the insulation slag bag, and rock wool fiber, borax pentahydrate and CaF are added. 2 Adjust the melt viscosity and keep the melt at a process temperature of 1480°C. During the holding period, remove the scum and bubbles in the melt to make the melt fully clarified and homogenized.

[0073] 3) Casting mold pretreatment: Before casting, quartz sand is lined inside the centrifugal casting machine pipe mold as a coating; then a hollow cylindrical wire mesh with a diameter slightly smaller than the inner diameter of the mold is placed in the mold and fixed at a position 20 mm away from the inner surface of the centrifugal casting machine mold through a preset groove inside the mold;

[0074] 4) Casting: The melt temperature is controlled at 1200°C, at which the high-temperature melt viscosity is approximately 3.5 Pa·s; the melt is poured into a preheated mold at a mold speed of 900 r / min to obtain a tube blank;

[0075] 5) Heat treatment of tube blank: After the tube blank is cooled to 750°C, it is demoulded and moved to a tunnel kiln for nucleation and crystallization treatment. The nucleation temperature is 700°C and the holding time is 2 hours; in the crystallization treatment, the crystallization temperature is 850°C and the holding time is 2 hours; then the tube blank after crystallization treatment is cooled in the furnace to obtain a cast stone tube;

[0076] 6) Pipeline finishing: The surface and inner wall of the cast stone pipe are cleaned, polished and ground to obtain the final product.

[0077] 7) The main chemical components of the cast stone pipe are: SiO 2 :44.48%, MgO: 24.28%, Fe 2 O 3 : 6.79%, Al2 O 3 :3.72%, CaO: 2.05%, Cr 2 O 3 :1.04%,Na 2 O: 1.53%;

[0078] 8) The main physical properties of the cast stone pipe are: Mohs hardness 9, alkali resistance (20% NaOH solution) 99.5%, acid resistance (98% H 2 SO 4 )98.8%, water absorption rate 0.030%, flexural strength 115Mpa, compressive strength 1179Mpa.

[0079] Comparative Example 1

[0080] 1) Raw material ratio: by mass percentage, 80% nickel iron slag, 20% borax pentahydrate (Na 2 B 4 O 7 10H 2 O);

[0081] 2) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into an insulation slag bag, and rock wool fiber and borax pentahydrate are added to adjust the melt viscosity. The slag and bubbles in the melt are removed during the insulation period to fully clarify and homogenize the melt.

[0082] 3) Casting mold pretreatment: Before casting, quartz sand is lined inside the centrifugal casting machine pipe mold as a coating; then a hollow cylindrical wire mesh with a diameter slightly smaller than the inner diameter of the mold is placed in the mold and fixed at a position 25 mm away from the inner surface of the centrifugal casting machine mold through a preset groove inside the mold;

[0083] 4) Casting: The melt temperature is controlled at 1300°C. At this time, the viscosity of the high-temperature melt is too high to be cast.

[0084] Comparative Example 2

[0085] 1) Raw material ratio: by mass percentage, 78% nickel iron slag, 15% rock wool fiber, 5% B 2 O 3 , 2% CaF 2 ;

[0086] 2) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into a heat-insulating slag bag, and a conditioning agent is added to adjust the melt viscosity. The slag and bubbles in the melt are removed during the heat-insulating period to make the melt fully clarified and homogenized.

[0087] 3) Casting mold pretreatment: Before casting, quartz sand is lined inside the centrifugal casting machine pipe mold as a coating; then a hollow cylindrical wire mesh with a diameter slightly smaller than the inner diameter of the mold is placed in the mold and fixed at a position 20 mm away from the inner surface of the centrifugal casting machine mold through a preset groove inside the mold;

[0088] 4) Casting: The melt temperature is controlled at 1200°C, at which time the high-temperature melt viscosity is approximately 3.7 Pa·s; the melt is poured into a preheated mold at a mold speed of 840 r / min to obtain a tube blank;

[0089] 5) Heat treatment of tube blank: After the tube blank is cooled to 600°C, it is demoulded and moved to a tunnel kiln for nucleation and crystallization treatment. The nucleation temperature is 550°C and the holding time is 0.5h; in the crystallization treatment, the crystallization temperature is 750°C and the holding time is 1h; then the tube blank after crystallization treatment is cooled at a speed of 10°C / min to obtain a cast stone tube;

[0090] 6) A large number of cracks appear on the surface of the obtained cast stone pipe, which does not meet the product requirements.

[0091] In summary, referring to the comparison between the above embodiments and the comparative examples, it can be understood that the present invention solves the following technical problems:

[0092] (1) By adding a small amount of tempering agent to control the viscosity of molten metallurgical slag (such as nickel-iron slag, chromium-iron slag, etc.) at the molding temperature (1100-1300°C), microcrystalline cast stone pipes can be directly made by centrifugal casting.

[0093] (2) By adjusting the heat treatment system such as crystallization temperature and nucleation temperature, the cast stone pipe is not easy to crack during the cooling, demoulding, crystallization and other processes, and a flawless product is obtained.

[0094] (3) Due to the adjustment of raw materials, the cast microcrystalline glass tube has better comprehensive performance than market competitors, and can achieve higher economic benefits at a lower production cost.

Claims

1. A method for directly producing cast stone pipes using molten metallurgical slag, characterized in that: The method comprises the following steps: (1) Melt viscosity adjustment and homogenization: High-temperature molten metallurgical slag is directly fed into a heat-insulating slag ladle, and a conditioning agent is added to adjust the melt viscosity. The raw material composition in the heat-insulating slag ladle is as follows: 5-30% conditioning agent and the rest is molten metallurgical slag; then, the slag is kept at 1430-1555°C for 30-120 minutes. During the heat-insulating period, the scum and bubbles of the melt are removed by stirring or adding a clarifier, so that the melt is fully clarified and the whole is homogenized; (2) Casting mold pretreatment: Before casting, a coating such as resin sand or a mold release agent is applied to the inside of the centrifugal casting machine pipe mold; then, a metal support structure is made into a cylindrical shape suitable for the mold, the diameter of the support structure is slightly smaller than the inner diameter of the mold and is placed in the mold, and fixed at a position 1 to 30 mm away from the inner surface of the centrifugal casting machine mold through a preset positioning structure inside the mold; (3) Casting: The melt temperature is controlled within the range of 1100 to 1300°C, and the high temperature melt viscosity is controlled within the range of 0.5 to 15 Pa·s; the melt is poured into a preheated mold by mobile casting, and centrifugally cast at a speed of 500 to 2000 rpm to obtain a tube blank; (4) Heat treatment of the tube blank: After the tube blank is cooled to the demoulding temperature, a demoulding device is used to separate the tube blank from the mold. The demoulding tube blank is moved to a tunnel kiln and subjected to nucleation and crystallization treatment at 600 to 1000° C. for 0.5 to 6 hours. The crystallized tube blank is then cooled at a uniform rate or cooled in the furnace to obtain a cast stone tube. (5) Pipe finishing: The surface and inner wall of the cast stone pipe are cleaned, polished and ground to obtain the final product.

2. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: In the step (1), the conditioning agent is divided into coal gangue, high-boron raw materials or other industrial waste residues and chemical reagents, wherein the high-boron raw materials are one or more mixtures of borax and high-boron tailings, the industrial waste residues are coal gangue, rock wool fibers, etc., the chemical reagents are calcium fluoride, boron oxide, etc.; the clarifier is one or more mixtures of industrial-grade antimony oxide and industrial-grade sodium chloride.

3. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: The molten metallurgical slag is selected from metallurgical waste slags such as nickel-iron slag, chromium-iron slag, vanadium-titanium blast furnace slag, etc. The molten slag is used at a temperature of 1500-1600° C. The clarifier accounts for 0-2% of the mass of the added conditioning agent.

4. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: In the step (3), the release agent is one of dry coatings selected from silica powder, diatomaceous earth or corundum powder; or a water-based coating made from the dry coating according to a certain ratio.

5. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: In the step (3), the pouring method is mobile pouring, and the pouring port is radially fed into the pipe mold at a uniform speed, wherein the direction in which the melt flows in should be tangent to the direction of rotation of the mold; The centrifugal casting machine is a horizontal centrifuge, the temperature range during centrifugal casting is 1100-1300°C, the rotation speed of the horizontal centrifuge is 500-2000 rpm, and the angle of centrifugal casting is 0-10°.

6. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: In the step (3), the melt viscosity of the high-temperature melt is controlled within the range of 0.5 to 5 Pa·s at 1200 to 1300° C.; and the melt viscosity is controlled within the range of 4 to 15 Pa·s at 1100 to 1200° C.

7. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: In the step (4), in the demolding treatment, the demolding temperature is 700-800°C; in the nucleation treatment, the nucleation temperature is 600-800°C, and the holding time is 0.5-3h; in the crystallization treatment, the crystallization temperature is 800-1000°C, and the holding time is 0.5-3h, and then the temperature is uniformly reduced at a rate of 2-10°C / min, or it is directly taken out when it is cooled to below 200°C in the furnace.

8. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 3, characterized in that: The conditioning agent is selected from at least one of SiO2, CaO, Al2O3, rock wool fiber, B2O3, CaF2, rock wool fiber, borax pentahydrate, and CaF2.

9. The method for directly preparing a cast stone pipe using molten metallurgical slag according to claim 1, characterized in that: In the step (1), the preset positioning structure inside the mold is a groove or a bracket.

10. A cast stone pipe prepared by the method of claim 1, characterized in that: The chemical composition of the cast stone pipe in the use state is as follows by mass percentage: MgO: 15% to 40%, Fe2O3: 1% to 10%, FeO: 1% to 5%, Al2O3: 2% to 8%, CaO: 8% to 25%, Cr2O3: 0.1% to 5%, Na2O and K2O: 0.1% to 3%, and the rest is SiO2.