Catalyst for sprayed concrete and preparation method thereof
Through the coordinated cooperation of water reducing agent, modified viscosity regulator and modified coagulation additive in sprayed concrete, the problem of excessive cement usage and difficult to control the rebound rate is solved, resource saving and performance improvement are achieved, and C25 is met Standard strength and construction quality of sprayed concrete.
Patent Information
- Application Number
- CN202411093953.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The amount of cement used in the existing jet concrete technology is too large, resulting in waste of resources and environmental pollution, and it is difficult to effectively control the rebound rate to meet the initial strength requirements.
Using a catalyst for spraying concrete, including a water reducer, a modified viscosity regulator, an ion chelating agent and a modified coagulation additive, by coordinating the percentage of each component and the preparation method, a suitable catalyst is formed, the amount of cement is reduced and the amount of cement is controlled. rebound rate.
It significantly reduces the amount of cement, meets the standard strength of C25 sprayed concrete, reduces the amount of quick-setting agent, reduces the rebound rate, and improves the construction quality and long-term mechanical properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of shotcrete admixtures, and in particular to a catalyst for shotcrete and a preparation method thereof. Background Art
[0002] Shotcrete is a construction method that uses a pressure spray gun to spray and pour fine stone concrete. It is often used to pour tunnel linings, walls, ceilings and other thin-walled structures or other structural linings and protective layers of steel structures. Wet shotcrete is powered by compressed air and uses concrete spraying machinery to mix raw materials such as cement, sand, stone, accelerator, admixture and water in a certain proportion into a mixture, which is transported through pipelines and sprayed at a high speed onto the surface of rock or concrete. Due to the unique use of wet shotcrete, in actual construction, the amount of shotcrete used is large and the cost is high.
[0003] As we all know, C25 shotcrete uses about 300 kg of cement per cubic meter to meet the design strength, but we currently use 440-500 kg / cubic meter; from the perspective of strength alone, it is a huge waste and is extremely environmentally unfriendly. The main purpose of increasing the amount of cement in the prior art is to enable the concrete to form initial strength faster, reduce block loss, and control the rebound rate. Therefore, people increase the amount of cement not to meet the design strength, but to control the rebound rate. Although the existing C25 shotcrete adopts the technical solution of increasing the amount of cement to achieve the purpose of controlling the rebound rate, it wastes a lot of cement and is not environmentally friendly. On this basis, the present invention proposes a catalyst for shotcrete and a preparation method thereof, which can meet the initial strength of concrete and effectively control the rebound rate on the basis of reducing the amount of cement. Summary of the invention
[0004] The main purpose of the present invention is to provide a catalyst for shotcrete and a preparation method thereof to solve the problems in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: A catalyst for shotcrete, comprising the following components by weight percentage: Water reducing agent 10-12%, modified viscosity regulator 0.3-0.5%, ion chelating agent 1-5%, modified coagulant aid 6-8%, air entraining agent 0.1-0.2%, and the balance is water.
[0006] Preferably, the preparation method of the modified viscosity modifier comprises the following steps: Add nano-silicon dioxide into a dispersing solvent for ultrasonic dispersion, and after uniform dispersion, input into a grinder for grinding for 10-15 minutes at a grinding speed of 1000-1500 r / min to obtain a grinding mixture; The coupling agent is added to deionized water to prepare an aqueous solution with a mass concentration of 3-6%, and the mixture is stirred at 800-1000 r / min for 5-8 minutes. Then, hydroxymethyl cellulose ether is added and ultrasonically mixed for 10-15 minutes to obtain a hydroxymethyl cellulose ether mixed solution. The ground mixture and the hydroxymethyl cellulose ether mixed solution are mixed evenly, reacted at 80-90° C. for 6-8 hours, and then placed in an oven and dried at 80-100° C. to obtain a modified viscosity regulator.
[0007] Further preferably, the dispersion solvent is anhydrous ethanol; The nano-silicon dioxide and the dispersing solvent are configured into an ethanol mixed solution with a mass concentration of 5-8%; The coupling agent is a silane coupling agent.
[0008] The silane coupling agent is methacryloxysilane.
[0009] Further preferably, the mass ratio of the nano-silica, the coupling agent and the hydroxymethyl cellulose ether is 1:0.1-0.3:1.2-2.
[0010] In the present invention, nano silicon dioxide is uniformly dispersed in anhydrous ethanol and then mixed with a mixed solution of a silane coupling agent and hydroxymethyl cellulose ether. The hydroxymethyl cellulose ether reacts with hydroxyl groups on the surface of the modified nano silicon dioxide to form hydrogen bonds, which are cross-linked into a network structure, thereby increasing the cohesive force of subsequent concrete and improving the viscosity and stability of the concrete.
[0011] Preferably, the preparation method of the modified coagulant aid comprises the following steps: Add an aluminum sulfate solution with a mass concentration of 20-25% to an aluminum hydroxide aqueous solution with a mass fraction of 10-15%, stir and mix, first react at 115-130°C for 3-3.5 hours, then react at 85-100°C for 4-5 hours, finally add a modifier, stir evenly to obtain a modified coagulant aid.
[0012] Further preferably, the molar ratio of aluminum sulfate to aluminum hydroxide is 0.8-1.2:1.
[0013] Further preferably, the modifier is a mixture of acetic acid and polyacrylamide in a mass ratio of 2-3:1.
[0014] The present invention modifies the coagulant and adopts a two-component system of aluminum sulfate and aluminum hydroxide in a molar ratio of (0.8-1.2):1. Compared with a single aluminum sulfate component (a molar ratio of aluminum to sulfate is 0.66), the two-component coagulant increases the aluminum content and reduces the sulfate content. The molar ratio of aluminum to sulfate in the coagulant is increased to 0.9-1.1, which can reduce the impact on the durability of concrete while ensuring the accelerating effect, thereby overcoming the limitations of the traditional single aluminum sulfate component to a certain extent.
[0015] Preferably, the water reducer is one of a polycarboxylate water reducer or a naphthalenesulfonate water reducer.
[0016] More preferably, the water reducer is a polycarboxylate water reducer.
[0017] Preferably, the ion chelating agent is one of EDTA, sodium tripolyphosphate or sodium gluconate.
[0018] Preferably, the air entraining agent is one of rosin-based air entraining agents, alkylbenzene sulfonates or fatty alcohol sulfonates.
[0019] Preferably, the air-entraining agent is a rosin-based air-entraining agent.
[0020] Further preferably, the air entraining agent is sodium rosinate.
[0021] Another object of the present invention is to provide a method for preparing a catalyst for shotcrete, comprising the following steps: Weigh the components according to the above weight percentages, including water reducing agent, modified viscosity modifier, ion chelating agent, modified coagulant aid, air entraining agent and water; The modified viscosity regulator is added into water, stirred evenly, and then a water reducer, an ion chelating agent, a modified coagulant aid and an air entraining agent are added in sequence, and stirred for 40-60 minutes at a rotation speed of 600-800 r / min to obtain the catalyst for shotcrete.
[0022] The present invention also provides application of the catalyst for shotcrete in C25 shotcrete.
[0023] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses a water reducing agent, a modified viscosity regulator, an ion chelating agent, a modified setting aid and an air entraining agent as raw materials, and coordinates the percentage of each component to prepare a catalyst dedicated to shotcrete C25. When used, it can not only reduce the amount of cement used in concrete to meet the standard strength of C25 shotcrete 28d, but also reduce the amount of accelerating setting agent, reduce the rebound rate, and is not easy to block the pipeline.
[0024] 2. The present invention can meet the initial strength of concrete and significantly and effectively control the rebound rate on the basis of reducing the amount of cement through the synergistic cooperation between the modified viscosity regulator and the modified coagulant aid.
[0025] 3. The catalyst of the present invention can significantly improve the construction quality of shotcrete, while ensuring the long-term mechanical properties and durability of the shotcrete. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to data. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not intended to limit the scope of the present invention in any way. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0027] All substances involved in the examples of the present invention are commercially available.
[0028] Example 1 The present embodiment provides a catalyst for shotcrete, comprising the following components in weight percentage: 10% water reducing agent, 0.3% modified viscosity regulator, 1% ion chelating agent, 6% modified coagulant aid, 0.1% air entraining agent, and the remainder water.
[0029] The water reducing agent is a polycarboxylate water reducing agent, the ion chelating agent is EDTA, and the air entraining agent is sodium rosinate.
[0030] The preparation method of the catalyst for shotcrete provided in this embodiment is as follows: S1. Preparation of modified viscosity modifier: S101. The nano-silica was added to anhydrous ethanol for ultrasonic dispersion at an ultrasonic power of 250w, and then uniformly dispersed and input into a grinder for grinding for 10min at a grinding speed of 1000r / min to obtain a grinding mixture; Wherein, the nano-silicon dioxide and the dispersing solvent are configured into an ethanol mixed solution with a mass concentration of 5%; S102. The silane coupling agent was added to deionized water to prepare a 3% aqueous solution, and stirred at 800 r / min for 5 min, and then hydroxymethyl cellulose ether was added and ultrasonically mixed for 10 min at an ultrasonic power of 250 w to obtain a hydroxymethyl cellulose ether mixture; Wherein, the mass ratio of the nano-silicon dioxide, the silane coupling agent and the hydroxymethyl cellulose ether is 1:0.1:1.2; S103. The ground mixture and the hydroxymethyl cellulose ether mixed solution are mixed evenly, reacted at 80° C. for 6 hours, and then placed in an oven and dried at 80° C. to obtain a modified viscosity regulator.
[0031] S2. Preparation of modified coagulant aid: Aluminum sulfate solution with a mass concentration of 20% is added to aluminum hydroxide with a mass fraction of 10%, and stirred evenly. The mixture is first reacted at 115°C for 3 hours, then at 85°C for 4 hours, and finally a modifier is added and stirred evenly to obtain a modified coagulant. The equivalent ratio of aluminum hydroxide to aluminum sulfate is 1:1; and the modifier is a mixture of acetic acid and polyacrylamide in a mass ratio of 2:1.
[0032] S3. Preparation of catalyst for shotcrete: Weigh the components according to the above amounts, add the modified viscosity regulator into the water, stir evenly, then add the water reducer, ion chelating agent, modified coagulant aid and air entraining agent in sequence, stir at a speed of 600r / min for 40 minutes to obtain the catalyst for shotcrete.
[0033] Example 2 The present embodiment provides a catalyst for shotcrete, comprising the following components in percentage by weight: 12% of a water reducing agent, 0.5% of a modified viscosity regulator, 5% of an ion chelating agent, 8% of a modified coagulant aid, 0.2% of an air entraining agent, and the remainder being water.
[0034] The water reducer is a polycarboxylate water reducer, the ion chelating agent is sodium gluconate, and the air entraining agent is sodium rosinate.
[0035] The preparation method of the catalyst for shotcrete provided in this embodiment is as follows: S1. Preparation of modified viscosity modifier: S101. The nano-silica was added to anhydrous ethanol for ultrasonic dispersion at an ultrasonic power of 250w, and then uniformly dispersed and input into a grinder for grinding for 15min at a grinding speed of 1500r / min to obtain a grinding mixture; Wherein, the nano-silicon dioxide and the dispersing solvent are configured into an ethanol mixed solution with a mass concentration of 8%; S102. The silane coupling agent was added to deionized water to prepare a 6% aqueous solution, and stirred at 1000 r / min for 8 min, and then hydroxymethyl cellulose ether was added and ultrasonically mixed for 15 min at an ultrasonic power of 250 w to obtain a hydroxymethyl cellulose ether mixture; Wherein, the mass ratio of the nano-silicon dioxide, the silane coupling agent and the hydroxymethyl cellulose ether is 1:0.3:2; S103. The ground mixture and the hydroxymethyl cellulose ether mixed solution are mixed evenly, reacted at 90° C. for 8 hours, and then placed in an oven and dried at 100° C. to obtain a modified viscosity regulator.
[0036] S2. Preparation of modified coagulant aid: Aluminum sulfate solution with a mass concentration of 25% is added to aluminum hydroxide with a mass fraction of 15%, and stirred evenly. The mixture is first reacted at 130°C for 3.5 hours, then reacted at 100°C for 5 hours, and finally a modifier is added and stirred evenly to obtain a modified coagulant. The equivalent ratio of aluminum hydroxide to aluminum sulfate is 1:1; and the modifier is a mixture of acetic acid and polyacrylamide in a mass ratio of 2:1.
[0037] S3. Preparation of catalyst for shotcrete: Weigh the components according to the above weight percentage, add the modified viscosity regulator into the water, stir evenly, then add the water reducer, ion chelating agent, modified coagulant aid and air entraining agent in sequence, stir at a speed of 800 r / min for 60 minutes to obtain the catalyst for shotcrete.
[0038] Example 3 The present embodiment provides a catalyst for shotcrete, comprising the following components in weight percentage: 11% of a water reducing agent, 0.4% of a modified viscosity regulator, 3% of an ion chelating agent, 7% of a modified coagulant aid, 0.15% of an air entraining agent, and the remainder being water.
[0039] The water reducing agent is a polycarboxylate water reducing agent, the ion chelating agent is EDTA, and the air entraining agent is sodium rosinate.
[0040] The preparation method of the catalyst for shotcrete provided in this embodiment is as follows: S1. Preparation of modified viscosity modifier: S101. The nano-silica was added to anhydrous ethanol for ultrasonic dispersion at an ultrasonic power of 250w, and then uniformly dispersed and input into a grinder for grinding for 15min at a grinding speed of 1500r / min to obtain a grinding mixture; Wherein, the nano-silicon dioxide and the dispersion solvent are configured into an ethanol mixed solution with a mass concentration of 6%; S102. The silane coupling agent was added to deionized water to prepare a 5% aqueous solution, and stirred at 900 r / min for 6 min, and then hydroxymethyl cellulose ether was added and ultrasonically mixed for 12 min at an ultrasonic power of 250 w to obtain a hydroxymethyl cellulose ether mixture; Wherein, the mass ratio of the nano-silicon dioxide, the silane coupling agent and the hydroxymethyl cellulose ether is 1:0.2:1.6; S103. The ground mixture and the hydroxymethyl cellulose ether mixed solution are mixed evenly, reacted at 85° C. for 7 hours, and then placed in an oven and dried at 90° C. to obtain a modified viscosity regulator.
[0041] S2. Preparation of modified coagulant aid: A 20% aluminum sulfate solution is added to a 10% aluminum hydroxide solution, stirred evenly, reacted at 120°C for 3.5 hours, then at 90°C for 4.5 hours, and finally a modifier is added and stirred evenly to obtain a modified coagulant. The equivalent ratio of aluminum hydroxide to aluminum sulfate is 1:1; and the modifier is a mixture of acetic acid and polyacrylamide in a mass ratio of 2.5:1.
[0042] S3. Preparation of catalyst for shotcrete: Weigh the components according to the above amounts, add the modified viscosity regulator into the water, stir evenly, then add the water reducer, ion chelating agent, modified coagulant aid and air entraining agent in sequence, stir at a speed of 700 r / min for 50 minutes to obtain the catalyst for shotcrete.
[0043] Comparative Example 1 This comparative example is substantially the same as Example 3, except that no nano-silicon dioxide is added when preparing the modified viscosity modifier, and the rest is the same as Example 3.
[0044] Comparative Example 2 This comparative example is substantially the same as Example 3, except that no dispersing solvent, anhydrous ethanol, is added when preparing the modified viscosity modifier. Others are the same as Example 3.
[0045] Comparative Example 3 This comparative example is substantially the same as Example 3, except that no grinding mixture is added when preparing the modified viscosity modifier, and the rest is the same as Example 3.
[0046] Comparative Example 4 This comparative example is substantially the same as Example 3, except that hydroxymethyl cellulose ether is directly used instead of the modified viscosity modifier, and the rest is the same as Example 3.
[0047] Comparative Example 5 This comparative example is basically the same as Example 3, except that acetic acid is used alone as the modifier, and the rest is the same as Example 3.
[0048] Comparative Example 6 This comparative example is basically the same as Example 3, except that polyacrylamide is used alone as the modifier, and the rest is the same as Example 3.
[0049] Comparative Example 7 This comparative example is basically the same as Example 3, except that no modifier is added, and the rest is the same as Example 3.
[0050] Comparative Example 8 This comparative example is basically the same as Example 3, except that the modified coagulant aid adopts a single-component system of aluminum sulfate, and the rest is the same as Example 3.
[0051] Concrete performance test: The rebound rate and compressive strength of shotcrete are tested according to the shotcrete rebound rate test method, shotcrete specimen preparation method and compressive strength test method in the "Technical Code for Application of Shotcrete" (JGJ / T372) standard.
[0052] 1.1 The catalysts of Examples 1-3 and Comparative Examples 1-8 of the present invention were used to prepare C25 shotcrete. The mix ratio of the C25 shotcrete is shown in Table 1.
[0053] Table 1 Concrete mix ratio
[0054] In Table 1, the admixtures include a catalyst and an accelerator, the accelerator is an alkali-free type, the dosage of the catalyst is 1%, and the average dosage of the accelerator is 3.96%.
[0055] 1.2 The existing polycarboxylate water reducer is used to prepare C25 shotcrete. The mix ratio of the concrete is shown in Table 2.
[0056] Table 2 Concrete mix ratio
[0057] In Table 2, the admixtures include water reducing agent and accelerating setting agent, and the average accelerating setting agent dosage is 6.36%.
[0058] 1.3 C25 shotcrete was prepared using the catalysts of Examples 1-3 and Comparative Examples 1-8 of the present invention, and performance tests were performed. The results are shown in Table 3.
[0059] Table 3 Performance test results
[0060] It can be seen from the data in Table 3 that the shotcrete prepared by the catalysts of Examples 1-3 of the present invention meets the standard strength of C25 shotcrete after 28 days of curing, and the average rebound rate of the prepared C25 shotcrete is between 5.2% and 5.5%; in Comparative Examples 1-3, one component of the modified viscosity modifier in the catalyst of the present invention is changed, and the performance of the prepared shotcrete is significantly lower than that of Example 3 of the present invention; in Comparative Examples 5-7, one component of the modified coagulant in the catalyst of the present invention is changed, and the performance of the prepared shotcrete is significantly lower than that of Example 3 of the present invention; and in Comparative Example 4, the modified viscosity modifier of the catalyst of the present invention adopts hydroxymethyl cellulose ether, and the performance of the prepared shotcrete is far lower than that of Example 3 of the present invention; and in Comparative Example 8, the modified coagulant of the catalyst of the present invention adopts a single-component system of aluminum sulfate, and the performance of the prepared shotcrete is far lower than that of Example 3 of the present invention. It can be seen that the catalyst of the present invention can significantly reduce the rebound rate of shotcrete and enhance the compressive strength of concrete.
[0061] According to the data analysis of Tables 1 to 3, the rebound rate of C25 shotcrete prepared by the existing polycarboxylate water-reducing agent is 9.72%, and the amount of accelerating agent is 6.36%, while the rebound rate of concrete prepared by the catalyst of Example 3 of the present invention is 5.2%, and the amount of accelerating agent is 3.96%; it can be seen that the concrete prepared by using the catalyst of the present invention greatly reduces the amount of cement, while meeting the C25 design strength, and reduces the amount of accelerating agent, reduces the rebound rate, reduces the loss of concrete and reduces the construction cost.
[0062] In summary, the present invention uses the synergistic combination of the modified viscosity regulator and the modified coagulant to enable the prepared catalyst to meet the initial strength of concrete while reducing the amount of cement when configuring C25 shotcrete, and to significantly and effectively control the rebound rate.
[0063] The above embodiments are only preferred technical solutions of the present invention and should not be regarded as limiting the present invention. The protection scope of the present invention shall be the technical solutions recorded in the claims, including equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.
Claims
1. A catalyst for shotcrete, characterized in that: The composition comprises the following components in percentage by weight: 10-12% of water reducing agent, 0.3-0.5% of modified viscosity adjusting agent, 1-5% of ion chelating agent, 6-8% of modified coagulant aid, 0.1-0.2% of air entraining agent and the balance of water.
2. A catalyst for shotcrete according to claim 1, characterized in that: The preparation method of the modified viscosity modifier comprises the following steps: Add nano-silicon dioxide into a dispersing solvent for ultrasonic dispersion, and after uniform dispersion, input into a grinder for grinding for 10-15 minutes at a grinding speed of 1000-1500 r / min to obtain a grinding mixture; The coupling agent is added to deionized water to prepare an aqueous solution with a mass concentration of 3-6%, and the mixture is stirred at 800-1000 r / min for 5-8 minutes. Then, hydroxymethyl cellulose ether is added and ultrasonically mixed for 10-15 minutes to obtain a hydroxymethyl cellulose ether mixed solution. The ground mixture and the hydroxymethyl cellulose ether mixed solution are mixed evenly, reacted at 80-90° C. for 6-8 hours, and then placed in an oven and dried at 80-100° C. to obtain a modified viscosity regulator.
3. A catalyst for shotcrete according to claim 2, characterized in that: The dispersing solvent is anhydrous ethanol; the coupling agent is a silane coupling agent, and the silane coupling agent is methacryloxysilane.
4. A catalyst for shotcrete according to claim 2, characterized in that: The nano silicon dioxide and the dispersing solvent are configured into an ethanol mixed solution with a mass concentration of 5-8%.
5. A catalyst for shotcrete according to claim 2, characterized in that: The mass ratio of the nano silicon dioxide, the coupling agent and the hydroxymethyl cellulose ether is 1:0.1-0.3:1.2-2.
6. A catalyst for shotcrete according to claim 1, characterized in that: The preparation method of the modified coagulant aid comprises the following steps: Add an aluminum sulfate solution with a mass concentration of 20-25% to an aluminum hydroxide aqueous solution with a mass fraction of 10-15%, stir and mix, first react at 115-130°C for 3-3.5 hours, then react at 85-100°C for 4-5 hours, finally add a modifier, stir evenly to obtain a modified coagulant aid.
7. A catalyst for shotcrete according to claim 6, characterized in that: The molar ratio of the aluminum sulfate to the aluminum hydroxide is 0.8-1.2:
1.
8. A catalyst for shotcrete according to claim 6, characterized in that: The modifier is a mixture of acetic acid and polyacrylamide, with a mass ratio of 2-3:
1.
9. A catalyst for shotcrete according to claim 1, characterized in that: The water reducer is one of a polycarboxylate water reducer or a naphthalenesulfonate water reducer; The ion chelating agent is one of EDTA, sodium tripolyphosphate or sodium gluconate; The air entraining agent is one of rosin-based air entraining agents, alkylbenzene sulfonates or fatty alcohol sulfonates.
10. A method for preparing a catalyst for shotcrete according to any one of claims 1 to 9, characterized in that: The steps include: Weigh the components according to the above weight percentages, including water reducing agent, modified viscosity modifier, ion chelating agent, modified coagulant aid, air entraining agent and water; The modified viscosity regulator is added into water, stirred evenly, and then a water reducer, an ion chelating agent, a modified coagulant aid and an air entraining agent are added in sequence, and stirred for 40-60 minutes at a rotation speed of 600-800 r / min to obtain the catalyst for shotcrete.
Citation Information
Patent Citations
Pervious concrete additive and pervious concrete
CN107686274A
Water reducer for sprayed concrete and preparation method thereof
CN107759126A
Sulfate-corrosion-resistant concrete and preparation method thereof
CN112279590A
High-strength colored concrete and preparation method thereof
CN112979237A
Anti-seepage accelerator and preparation method therefor
WO2024152438A1