Variable-temperature coordinated elastic concrete material as well as preparation method and application thereof

Through the use of two-component water-based polyurethane materials, the cracking problem of concrete structures under temperature fatigue stress in plateau areas is solved, the ultimate strain rate and elastic energy absorption effect of concrete are improved, the preparation process is simplified, and the use of polyurethane materials is reduced. , realizes the efficient crack-proof performance of concrete under large temperature difference environment.

CN118955048APending Publication Date: 2024-11-15RAILWAY CONSTR RES INST OF CHINA ACAD OF RAILWAY SCI CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411050489.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art cannot effectively prevent surface cracking under temperature fatigue stress in concrete structures in plateau areas, and the preparation process of polyurethane composite concrete is complicated and easy to foam, affecting strength.

Method used

Using two-component water-based polyurethane material, the aqueous highly elastic polyurethane emulsion is uniformly mixed by uniform mixing of water-based polyurethane group A and water-based polyurethane group B at a mass ratio of 100: (40-50), and stirred with cement, sand, gravel and other materials. Add water-reducing and defoaming functional components to prepare temperature-coordinated elastic concrete with high elasticity, ultimate strain and adjustable modulus.

Benefits of technology

It significantly improves the ultimate strain rate and elastic energy absorption effect of concrete, reduces the number of cracks, avoids cracking in concrete structures under large temperature differences, and reduces the amount of polyurethane materials, simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974763780000071
    Figure BDA0004974763780000071
Patent Text Reader

Abstract

The invention discloses a variable-temperature coordinated elastic concrete material as well as a preparation method and application thereof. The concrete is prepared from the following raw materials: cement, machine-made sand, 5-10mm graded broken stone, 10-20mm graded broken stone, a waterborne polyurethane group A, a waterborne polyurethane group B, a water-reducing and defoaming functional component and water. The waterborne polyurethane modified concrete with the characteristic that the modulus is controllable along with the temperature from low-temperature high modulus to high-temperature low modulus is prepared by utilizing the characteristics that the waterborne polyurethane is high in elasticity and the modulus is controllable along with the temperature, and when the environment temperature is increased by 40 DEG C, the elastic modulus of the variable-temperature coordinated elastic concrete is reduced by 15.40%-23.56%; compared with a conventional concrete material, the elastic energy absorption effect of the waterborne polyurethane modified concrete is improved by 99.47%-239.06%, the limit strain rate is improved by 180.00%-245.45%, the number of cracks is obviously reduced along with increase of the mixing amount of the two-component waterborne polyurethane, and the anti-cracking effect of a concrete structure in a large-temperature-difference environment is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of concrete materials, and in particular to a temperature-variable coordinated elastic concrete material and a preparation method and application thereof. Background Art

[0002] The altitude of plateau areas is generally above 500m. The highest city in the Qinghai-Tibet Plateau, Lhasa, has an altitude of 3,650m. Its unique alpine climate environment features low ambient air pressure, large daily temperature difference, low ambient temperature, and strong solar radiation. The excessive temperature difference between day and night and solar radiation cause the concrete structure to gradually crack after demolding, which becomes a major challenge for concrete structures in service in plateau areas.

[0003] In order to solve the cracking problem of concrete structures, the patent "Anti-crack concrete and its production and preparation method (CN202211420580.0)" invented anti-crack concrete using anti-crack fibers, lignin and other materials, which improved the toughness of concrete and enhanced the crack resistance of concrete. The patent "Modified polyester fiber (CN202010403791.8)" invented a kind of anti-crack concrete using modified polyester fiber. The patent "A kind of high temperature resistant crack-resistant concrete and its preparation method (CN202011098738.8)" invented a kind of high temperature resistant crack-resistant concrete using nano-titanium dioxide, nano-silicon dioxide, nano-carbon fiber and graphene, which improved the high temperature resistance and compressive strength of concrete, increased the toughness of concrete and thus reduced the generation of microcracks, but the cost of its raw materials is too high. Existing research often uses fiber toughening technology to improve the crack resistance of concrete. The prepared fiber concrete material has the advantages of high strength, high toughness, and good deformation coordination. However, this method only improves the strength and toughness of concrete under load, and does not significantly improve the crack resistance of the concrete surface under temperature fatigue stress.

[0004] As a high-strength elastic material, polyurethane has the advantages of low density, high strength, high stiffness and controllable elastic deformation with temperature. Its main components are polyol (HO-R-OH) and polyisocyanate (OCN-R'-NCO). The two functional groups form an extended chain and network through the urethane bond formed by the exothermic reaction, which makes polyurethane have adjustable mechanical and deformation properties. The patent "Polyurethane composite concrete material for bridge deck pavement and use method (CN201611209256.9)" invented a polyurethane composite concrete material for bridge deck pavement. The invention improves the strength of the concrete structure, but the polyurethane used is a single-component polyurethane. When using the polyurethane composite concrete, all raw materials need to be mixed on site, which is troublesome to operate. In addition, this type of polyurethane composite concrete cannot come into contact with water and cannot exert the strength advantage of cement reaction to generate hydration products. The patent "Two-component polyurethane composition for concrete modification and preparation method thereof (CN201911273866.9)" invented two-component polyurethane modified concrete, which solved the problem of on-site mixing of polyurethane materials during the preparation of polyurethane concrete and reduced the difficulty of preparation. However, since no hydrophilic chain extender is added to the two-component polyurethane, there is still the problem of easy foaming of polyurethane after contact with water, which affects the strength of concrete.

[0005] Therefore, how to provide a temperature-controlled elastic concrete material and a preparation method suitable for large temperature difference environments is an urgent problem that technicians in this field need to solve. Summary of the invention

[0006] In view of this, the present invention provides a temperature-variable coordinated elastic concrete material and a preparation method and application thereof. The temperature-variable coordinated elastic concrete prepared by utilizing the high elasticity, high tensile strain and adjustable elastic modulus of waterborne polyurethane has the characteristics of strong elastic energy absorption capacity, high ultimate strain and good tensile performance, and has the unique property of "low temperature high modulus - high temperature low modulus" that the modulus can be controlled with temperature, which can effectively prevent surface cracking of concrete structures under the action of temperature fatigue stress.

[0007] In order to achieve the above object, the technical solution of the present invention is:

[0008] A variable temperature coordinated elastic concrete material suitable for large temperature difference environment, comprising the following raw material components in the following amounts: cement 300kg / m 3 ~600kg / m 3 , Machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3~800kg / m 3 , Waterborne polyurethane group A 10kg / m 3 ~50kg / m 3 , Waterborne polyurethane group B 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 , water 50kg / m 3 ~200kg / m 3 .

[0009] Furthermore, the gradation of the machine-made sand should be within the limit range of zone II machine-made sand, and the stone powder content should not exceed 10%.

[0010] Furthermore, the waterborne polyurethane group A comprises the following raw materials in parts by weight: 30 to 80 parts of macromolecular diol, 30 to 60 parts of hydrophilic chain extender, 1 to 10 parts of ethylene oxide, 1 to 5 parts of organic tin compound, and 1 to 5 parts of antioxidant.

[0011] Furthermore, the macromolecular diol is a polyether or polyester diol, the molecular weight of which is 2000-5000 and the hydroxyl value is 50mg / g-150mg / g; and the organic tin compound is dibutyltin dilaurate or stannous octoate.

[0012] Furthermore, the hydrophilic chain extender is one of dimethylol propionic acid or dimethylol butyric acid or a mixture of the two; the antioxidant is 2,6-di-tert-butyl-4-methylphenol or tri-tert-butyl hydroxybenzoate.

[0013] Furthermore, the waterborne polyurethane group B comprises the following raw materials in parts by weight: 60 to 90 parts of diisocyanate and 10 to 20 parts of organic amine compound.

[0014] Furthermore, the diisocyanate is an aliphatic diisocyanate; and the organic amine compound is triethylamine or diethylenetriamine.

[0015] The present invention also discloses a method for preparing the above-mentioned variable temperature coordinated elastic concrete material suitable for a large temperature difference environment, which is characterized by comprising the following steps:

[0016] Step 1, uniformly mixing waterborne polyurethane group A and waterborne polyurethane group B at a mass ratio of 100:(40-50) to prepare a waterborne high elastic polyurethane emulsion;

[0017] Step 2: Put the water-based high elastic polyurethane emulsion and graded crushed stone into a mixer and mix them;

[0018] Step 3: Add cement and machine-made sand into a mixer and mix for 1 minute;

[0019] Step 4: Add mixing water and water-reducing and defoaming functional components into a mixer for mixing and stirring, and obtain variable temperature coordinated elastic concrete after the materials are evenly mixed.

[0020] Furthermore, the solid content of the water-based high-elastic polyurethane emulsion is 30% to 50%, and the amount added to the concrete is 10% to 20%.

[0021] It can be seen from the above technical solutions that, compared with the prior art, the present invention discloses a variable temperature coordinated elastic concrete material and a preparation method and application thereof, which have the following beneficial effects:

[0022] 1. The two-component hydrophilic polyurethane material of the present invention can be mixed with water without foaming, and the two-component hydrophilic polyurethane material can be directly used as a cementitious material in the preparation of concrete, which greatly reduces the difficulty of applying polyurethane concrete. At the same time, cement and other cementitious materials in the polyurethane modified concrete material of the present invention can undergo hydration reaction, giving full play to the coagulation and hardening effect of the cementitious material, saving the amount of polyurethane material.

[0023] 2. After modification with two-component water-based polyurethane, the ultimate strain rate of the temperature-controlled elastic concrete increased by 180.00% to 245.45% with little change in strength, and the elastic energy absorption effect increased by 99.47% to 239.06%. The number of cracks decreased significantly with the increase in the dosage of two-component water-based polyurethane. When the dosage of two-component water-based polyurethane is above 10%, cracks in the concrete structure will be avoided in a large temperature difference environment.

[0024] 3. The variable temperature coordinated elastic concrete shows the characteristic of "high modulus at low temperature - low modulus at high temperature" that the modulus can be controlled with temperature. When the ambient temperature increases by 40°C, the elastic modulus of the variable temperature coordinated elastic concrete decreases by 15.40% to 23.56%, indicating that when the ambient temperature is too high, the variable temperature coordinated elastic concrete can improve its deformation coordination ability by reducing the elastic modulus, thereby further avoiding plastic cracking of the concrete. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] The present invention designs a variable temperature coordinated elastic concrete material and its preparation method and application. The raw materials are: cement 300kg / m 3 ~600kg / m 3 , Machine-made sand 400kg / m3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m 3 , waterborne polyurethane (Group A) 10kg / m 3 ~50kg / m 3 , waterborne polyurethane (Group B) 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 , water 50kg / m 3 ~200kg / m 3 .

[0027] Example 1

[0028] The raw material quality ratio of waterborne polyurethane component A used in variable temperature coordinated elastic concrete is as follows:

[0029] Polyester diol (molecular weight 4000, hydroxyl value 100 mgKOH / g): 2,2-dihydroxymethylpropionic acid: ethylene oxide: dibutyltin dilaurate: 2,6-di-tert-butyl-4-methylphenol = 50:40:3:1:2.

[0030] The quality ratio of the raw materials of waterborne polyurethane component B used in variable temperature coordinated elastic concrete is as follows:

[0031] Toluene diisocyanate: diethylenetriamine = 75:15.

[0032] The temperature-controlled elastic concrete based on polyurethane modification technology has the following raw material mix:

[0033] 1m 3 The raw materials are as follows: 430 kg of ordinary silicate with P·O 42.5; 604 kg of machine-made sand with a fineness modulus of 2.8 and grading zone II; 330 kg of crushed stone with a diameter of 5 mm to 10 mm; 770 kg of crushed stone with a diameter of 5 mm to 10 mm; 14.33 kg of water-based polyurethane (group A); 7.17 kg of water-based polyurethane (group B); 0.5 kg of water-reducing and defoaming functional component (ZM-1B naphthalene-based high-efficiency water-reducing agent: BYK-1796 silicone defoaming agent = 4:1); and 161 kg of water.

[0034] The preparation method is implemented according to the following steps:

[0035] Step 1: uniformly mix the prepared waterborne polyurethane components A and B at a mass ratio of 100:50 to prepare a waterborne high elastic polyurethane emulsion with a solid content of 50%;

[0036] Step 2: Put the water-based high elastic polyurethane emulsion and aggregate into a mixer and continue mixing for 2 minutes;

[0037] Step 3: Put cement and other cementitious materials into the mixer and continue mixing for 1 minute;

[0038] Step 4: Add mixing water and water-reducing and defoaming functional components into a mixer and continue mixing and stirring for 3 minutes. After the materials are evenly mixed, variable temperature coordinated elastic concrete is obtained.

[0039] Example 2

[0040] The raw material quality ratio of waterborne polyurethane component A used in variable temperature coordinated elastic concrete is as follows:

[0041] Polyester diol (molecular weight 4000, hydroxyl value 100 mgKOH / g): 2,2-dihydroxymethylpropionic acid: ethylene oxide: dibutyltin dilaurate: 2,6-di-tert-butyl-4-methylphenol = 50:40:3:1:2.

[0042] The quality ratio of the raw materials of waterborne polyurethane component B used in variable temperature coordinated elastic concrete is as follows:

[0043] Toluene diisocyanate: diethylenetriamine = 75:15.

[0044] The temperature-controlled elastic concrete based on polyurethane modification technology has the following raw material mix:

[0045] 1m 3 The raw materials contained are as follows: 430 kg of P·O 42.5 ordinary silicate; 604 kg of machine-made sand with a fineness modulus of 2.8 and grading zone II; 1100 kg of crushed stone with a diameter of 5 mm to 10 mm; 28.67 kg of water-based polyurethane (group A); 14.33 kg of water-based polyurethane (group B); 0.3 kg of water-reducing and defoaming functional components (ZM-1B naphthalene-based high-efficiency water-reducing agent: BYK-1796 defoaming agent = 4:1); and 151 kg of water.

[0046] The preparation method is implemented according to the following steps:

[0047] Step 1, uniformly mixing the prepared waterborne polyurethane components A and B at a mass ratio of 100:50 to prepare a waterborne high elastic polyurethane emulsion with a solid content of 55%;

[0048] Step 2: Put the water-based high elastic polyurethane emulsion and aggregate into a mixer and continue mixing for 2 minutes;

[0049] Step 3: Put cement and machine-made sand cementitious materials into a mixer and continue mixing for 1 minute;

[0050] Step 4: Add mixing water and water-reducing and defoaming functional components into a mixer and continue mixing and stirring for 3 minutes. After the materials are evenly mixed, variable temperature coordinated elastic concrete is obtained.

[0051] Example 3

[0052] The raw material quality ratio of waterborne polyurethane component A used in variable temperature coordinated elastic concrete is as follows:

[0053] Polyester diol (molecular weight 4000, hydroxyl value 100 mgKOH / g): 2,2-dihydroxymethylpropionic acid: ethylene oxide: dibutyltin dilaurate: 2,6-di-tert-butyl-4-methylphenol = 50:40:3:1:2.

[0054] The quality ratio of the raw materials of waterborne polyurethane component B used in variable temperature coordinated elastic concrete is as follows:

[0055] Toluene diisocyanate: diethylenetriamine = 75:15.

[0056] The temperature-controlled elastic concrete based on polyurethane modification technology has the following raw material mix:

[0057] 1m 3 The raw materials are as follows: 430 kg of ordinary silicate with a P·O 42.5; 604 kg of machine-made sand with a fineness modulus of 2.8 and grading zone II; 1100 kg of crushed stone with a size of 5 mm to 10 mm; 43.00 kg of water-based polyurethane (group A); 21.50 kg of water-based polyurethane (group B); 0.2 kg of water-reducing and defoaming functional components (ZM-1B naphthalene-based high-efficiency water-reducing agent: BYK-1796 defoaming agent = 4:1); and 140 kg of water.

[0058] The preparation method is implemented according to the following steps:

[0059] Step 1, uniformly mixing the prepared waterborne polyurethane components A and B at a mass ratio of 100:50 to prepare a waterborne high elastic polyurethane emulsion with a solid content of 55%;

[0060] Step 2: Put the water-based high elastic polyurethane emulsion and aggregate into a mixer and continue mixing for 2 minutes;

[0061] Step 3: Put cement and other cementitious materials into the mixer and continue mixing for 1 minute;

[0062] Step 4: Add mixing water and water-reducing and defoaming functional components into a mixer and continue mixing and stirring for 3 minutes. After the materials are evenly mixed, variable temperature coordinated elastic concrete is obtained.

[0063] Comparative Example 1

[0064] A method for preparing conventional C40 concrete, the raw material ratio is as follows:

[0065] 1m 3 The raw materials in C40 concrete are: 430 kg of P·O 42.5 ordinary Portland cement; 604 kg of machine-made sand with a fineness modulus of 2.8 and grading zone II; 1100 kg of 5 mm to 10 mm crushed stone; 172 kg of water; and 3 kg of ZM-1B naphthalene-based high-efficiency water reducer.

[0066] Preparation method: Put cement, machine-made sand, coarse aggregate, water reducing agent and water into a mixer and stir and mix until the materials are evenly mixed to obtain conventional C40 concrete.

[0067] Table 2 shows the test results of compressive strength, flexural strength, elastic modulus at different temperatures, ultimate strain rate, elastic energy absorption effect and temperature fatigue crack resistance of the variable temperature coordinated elastic concrete in Examples 1 to 3 and the conventional C40 concrete in the comparative example.

[0068] Directions:

[0069] Table 2 Test results of variable temperature coordinated elastic concrete performance

[0070]

[0071] As can be seen from Table 2, the variable temperature coordinated elastic concrete prepared by the present invention can significantly improve the elastic energy absorption effect and the ultimate tensile strain rate of concrete under the premise of ensuring that the compressive and flexural strengths do not change much, compared with the conventional C40 concrete with the same proportion and without water-based polyurethane. This shows that the variable temperature coordinated elastic concrete prepared by the present invention can well delay the damage accumulation of concrete under the action of temperature fatigue stress, and reduce the risk of concrete cracking in a large temperature difference environment; at the same time, the variable temperature coordinated elastic concrete also shows the "low temperature high modulus-high temperature low modulus" characteristic that the elastic modulus of concrete gradually decreases with the increase of ambient temperature. When the surface temperature of the railway pier increases in the plateau with strong solar radiation, the modulus can be reduced, which can improve the ductility and deformation capacity of the outer layer of concrete, thereby avoiding the cracking of the concrete.

[0072] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A temperature-controlled elastic concrete material, characterized in that: The raw material components include the following amounts: cement 300kg / m 3 ~600kg / m 3 , Machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m 3 , Waterborne polyurethane group A 10kg / m 3 ~50kg / m 3 , Waterborne polyurethane group B 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 、Water 50kg / m 3 ~200kg / m 3 .

2. The variable temperature coordinated elastic concrete material according to claim 1, characterized in that: The gradation of the machine-made sand should be within the limit range of zone II machine-made sand, and the stone powder content should not exceed 10%.

3. The temperature-modulating elastic concrete material according to claim 1, characterized in that: The waterborne polyurethane group A comprises the following raw materials in parts by weight: 30 to 80 parts of macromolecular diol, 30 to 60 parts of hydrophilic chain extender, 1 to 10 parts of ethylene oxide, 1 to 5 parts of organic tin compound, and 1 to 5 parts of antioxidant.

4. The temperature-variable coordinated elastic concrete material according to claim 1, characterized in that: The macromolecular diol is a polyether or polyester diol, with a molecular weight of 2000-5000 and a hydroxyl value of 50mg / g-150mg / g; the organic tin compound is dibutyltin dilaurate or stannous octoate.

5. The temperature-variable coordinated elastic concrete material according to claim 4, characterized in that: The hydrophilic chain extender is one of dimethylol propionic acid and dimethylol butyric acid or a mixture of the two; the antioxidant is 2,6-di-tert-butyl-4-methylphenol or tri-tert-butyl hydroxybenzoate.

6. The variable temperature coordinated elastic concrete material suitable for large temperature difference environment according to claim 1, characterized in that: The waterborne polyurethane group B comprises the following raw materials in parts by weight: 60 to 90 parts of diisocyanate and 10 to 20 parts of organic amine compound.

7. The temperature-modulating elastic concrete material according to claim 6, characterized in that: The diisocyanate is an aliphatic diisocyanate; and the organic amine compound is triethylamine or diethylenetriamine.

8. The method for preparing a temperature-variable coordinated elastic concrete material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1, uniformly mixing waterborne polyurethane group A and waterborne polyurethane group B at a mass ratio of 100:(40-50) to prepare a waterborne high elastic polyurethane emulsion; Step 2: Put the water-based high elastic polyurethane emulsion and graded crushed stone into a mixer and mix them; Step 3: Add cement and machine-made sand into a mixer and mix for 1 minute; Step 4: Add mixing water and water-reducing and defoaming functional components into a mixer for mixing and stirring, and obtain variable temperature coordinated elastic concrete after the materials are evenly mixed.

9. The method for preparing a temperature-variable coordinated elastic concrete material according to claim 8, characterized in that: The solid content of the water-based high-elasticity polyurethane emulsion is 30% to 50%, and the admixture amount in the concrete is 10% to 20%.

10. Use of the variable temperature coordinated elastic concrete material according to any one of claims 1 to 7 in an environment with a large temperature difference between day and night.

Citation Information

Patent Citations

  • Polyurethane composite concrete material for bridge deck pavement and using method thereof

    CN106587727A

  • Two-component polyurethane composition for concrete modification and preparation method thereof

    CN110922091A

  • Anti-crack concrete

    CN111548087A

  • High-temperature-resistant anti-cracking concrete and preparation method thereof

    CN112321206A

  • Anti-crack concrete and production and preparation method thereof

    CN115893925A