Method for preparing autoclaved aerated concrete block by using furnace bottom slag and desulfurized sludge of coal-fired power plant

By using furnace bottom slag and desulfurized sludge to prepare autoclaved aerated concrete blocks, the problem of supply and treatment of raw materials is solved, resource utilization and cost reduction are achieved, and environmental benefits and product performance are improved.

CN118955067APending Publication Date: 2024-11-15CHANGXING TIANDA ENVIRONMENTAL PROTECTION BUILDING MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410964742.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the supply and demand imbalance of fly ash and desulfurization gypsum are problematic, as well as environmental protection and economic benefits caused by the difficulty of furnace bottom slag and desulfurization sludge.

Method used

The method of preparing autoclaved aerated concrete blocks in coal-fired power plant furnace bottom slag and desulfurization sludge is used to prepare autoclaved aerated concrete blocks through the processing and pouring process of raw materials, and the chemical composition of the glass body of the furnace bottom slag and the desulfurization sludge are used to replace some raw materials and reduce production. Cost and realize resource utilization.

Benefits of technology

The comprehensive utilization of solid waste is realized, the production cost of aerated concrete blocks is reduced, environmental protection problems are solved, and the utilization rate of raw materials and product performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955067A_ABST
    Figure CN118955067A_ABST
Patent Text Reader

Abstract

The invention relates to the field of preparation of autoclaved aerated concrete blocks, in particular to a method for preparing autoclaved aerated concrete blocks by using coal-fired power plant furnace bottom slag and desulfurized sludge, which comprises the following steps: S1, preparing raw materials; s2, raw material processing; s3, a mold oil coating section; s4, a pouring and burdening section: conveying and metering the slurry, lime powder, cement, aluminum paste and an additive, adding into a pouring stirrer, and uniformly stirring to prepare blank slurry; s5, standing and pre-curing section; s6, turning over the cutting section; s7, an autoclaved curing section; according to three requirements of innocent treatment, low carbon and resource utilization, the research and development of a production process for producing an autoclaved aerated concrete product from the furnace bottom slag and the desulfurized sludge are carried out, comprehensive utilization of solid waste is realized, the furnace bottom slag and the desulfurized sludge are turned into wealth, the problem of environmental protection can be solved, the production cost is greatly reduced, and the method is suitable for industrial production. And obvious economic benefits are brought.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of autoclaved aerated concrete block preparation, and in particular to a method for preparing autoclaved aerated concrete blocks by utilizing bottom slag and desulfurized sludge from a coal-fired power plant. Background Art

[0002] Fly ash autoclaved aerated concrete blocks use fly ash from power plants as the main raw material. They are widely used in the production of aerated concrete blocks. However, fly ash is also an important raw material for cement and concrete production. It is often in short supply. As a raw material for the production of aerated concrete blocks, it is not economically ideal. The bottom slag of a coal-fired power plant is the slag discharged from the bottom after the coal is burned in the boiler. Due to its high temperature, it is usually cooled with water and then discharged by the slag removal system. The moisture content is about 30%. It has been landfilled as solid waste for a long time, which not only occupies a large amount of farmland, but also pollutes the environment. Limestone-gypsum wet desulfurization is the most widely used process in flue gas desulfurization projects in thermal power plants. In order to ensure the normal operation of the desulfurization system, it is necessary to discharge desulfurization wastewater regularly. The treatment of a large amount of desulfurization wastewater will inevitably lead to the generation of a large amount of desulfurization sludge. Desulfurization sludge has the characteristics of high water content, high viscosity, and large fluctuations in chemical composition. Compared with ordinary sludge, it has high heavy metal content and high chloride ion content. It is easy to produce secondary pollution during the treatment process, which makes it difficult to treat it harmlessly.

[0003] At present, the main treatment methods for bottom ash and desulfurization sludge include landfill, incineration and composting. The landfill method needs to be gradually replaced because the harmful components of the sludge will cause groundwater pollution due to leakage, and the dust and odor problems in the landfill are prone to secondary pollution. The incineration method is prone to secondary pollution due to the production of fly ash, slag and flue gas during the incineration process. In addition, the sludge has a high water content and low calorific value, which requires a large amount of heat energy and is not conducive to the stable operation of the boiler. Sludge composting, as an agricultural method, is a process of fermentation using microorganisms in the sludge. The disadvantage is that the harmful components in the sludge are prone to cause secondary pollution and other problems, including heavy metals, pathogens, etc. Therefore, the current sludge disposal methods have certain limitations and there is a certain gap with the national environmental protection requirements.

[0004] In the prior art, two major raw materials for preparing autoclaved aerated concrete blocks are fly ash and desulfurized gypsum. For example, the patent with application number CN202110852008.0 discloses an autoclaved aerated concrete block and a preparation method thereof, and the patent with application number CN201510509221.6 discloses a method for manufacturing an autoclaved fly ash aerated concrete block. For example, the patent with application number CN201710636539.X discloses a fly ash-sand autoclaved aerated concrete block and a preparation method thereof. The raw materials for preparing autoclaved aerated concrete blocks in these patents all use fly ash and desulfurized gypsum, and the proportion of these two raw materials is often not small, which often leads to a phenomenon of supply exceeding demand, and the cost is also high. Bottom slag contains a high moisture content, a large loss on ignition, and the wear resistance and chemical composition of the bottom slag of different power plants fluctuate greatly, resulting in a low market value utilization rate and a low price. With the development of the aerated concrete block production industry, the demand for raw materials is increasing. The bottom slag contains more glass after water quenching in a high-temperature molten state, which has better activity and a high content of silicon dioxide in its chemical composition. If it can be used to its full potential and replace the siliceous materials in aerated concrete blocks, it will not only solve its environmental problems, but also bring obvious economic benefits. Desulfurization sludge has high heavy metal content and high chloride ion content, and is prone to secondary pollution during the treatment process. Therefore, it cannot be disposed of as ordinary sludge. Through laboratory analysis, the chemical composition of desulfurization sludge is mainly CaSiO4, which is close to the chemical composition of desulfurization gypsum in coal-fired power plants. Therefore, it can replace the desulfurization gypsum required in the production process of aerated concrete blocks for production, realizing waste into treasure. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention aims to provide a method for preparing autoclaved aerated concrete blocks using bottom slag and desulfurization sludge from coal-fired power plants and a casting method thereof, which solves the problems existing in the prior art, fully utilizes the chemical composition and physical property characteristics of bottom slag and desulfurization sludge, realizes the comprehensive utilization of solid waste, and broadens the range of raw materials for aerated concrete blocks. The desulfurization sludge contains part of the desulfurization gypsum, which can replace part of the retarder to a certain extent, play a role in adjusting the hardening speed of the green body, and reduce production costs.

[0007] (II) Technical solution

[0008] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a method for preparing autoclaved aerated concrete blocks using bottom slag and desulfurized sludge from a coal-fired power plant, characterized in that it comprises the following steps: S1, raw material preparation: the raw materials to be prepared include bottom slag, desulfurized sludge, cement, lime, aluminum paste, and admixtures; S2, raw material processing: the bottom slag and desulfurized sludge are made into slurry and stored in a slurry tank for standby use, the lime is ground into lime powder and stored in a lime bin for standby use, the cement is stored in a cement bin for standby use, the aluminum paste is stored in an aluminum paste storage tank for standby use, and the admixture is stored in an admixture storage tank for standby use; S3, mold oiling section: the release agent is evenly applied to each surface inside the mold; S4, pouring and batching section: the slurry, lime powder, cement, aluminum paste, and admixture are added into a pouring mixer through conveying and metering, and stirred evenly to prepare a green body slurry, wherein the proportions are made according to the following weight parts: 78 to 80 parts of slurry, 78 to 80 parts of lime, and 78 to 80 parts of aluminum paste. 8-10 parts of ash powder, 8-10 parts of cement, 0.08-0.1 parts of aluminum paste, and 0.03-0.06 parts of admixture; S5, static pre-curing section: put the prepared green body slurry into the mold, transport the mold by means of casting shuttle, static room traction machine and other equipment, transport the green body slurry to the static room for pre-curing process, pre-form the green body slurry into green body, and transport it to the designated position of the flip cutting section after the pre-curing is completed; S6, flip cutting section: put the pre-cured green body slurry into the mold, and transport it to the designated position of the flip cutting section after the pre-curing is completed; The blank and the mold are lifted by the turning hoist onto the cutting trolley, turned over and demoulded, and then cut to size by the longitudinal cutting machine and the transverse cutting machine; S7, autoclave curing section: the cut blank and the side plate loaded with the blank are carried by the autoclave trolley and transported to the autoclave for autoclave curing, and then transported to the section at the designated position of the packaging line; S8, palletizing and packaging section: the autoclave-cured blanks are palletized and packaged and transported to the workshop door for easy handling by forklift.

[0009] Preferably, the method for making the bottom ash and desulfurization sludge into slurry in step S2 is as follows: 1) the bottom ash is piled up in the yard to drain, and after its moisture content is reduced to below 25%, it is transported to the ball mill through a grab crane, a slag feed hopper, and a weighing belt conveyor; 2) the desulfurization sludge is transported to the ball mill through a grab crane; 3) the waste slurry is transported to the ball mill, and then the ball mill is started to grind the bottom ash and desulfurization sludge into slurry, wherein the weight ratio of the bottom ash, desulfurization sludge and waste slurry is: (75-80): (3-6): (55-65); 4) the prepared slurry is transported to a slurry tank for storage.

[0010] Preferably, the waste slurry is circulated and stored in the workshop through the waste slurry circulation section.

[0011] Preferably, the additive is a foam stabilizer.

[0012] Preferably, in step S4, the slurry, lime powder and cement are first added to the pouring mixing tank in sequence and stirred for 80 to 90 seconds, and then the aluminum paste is added and stirred for 10 to 12 seconds, and then the foam stabilizer is added and stirred for another 120 to 130 seconds.

[0013] Preferably, during step S4, steam is introduced into the pouring and stirring tank for heating, so that the temperature in the pouring and stirring tank is maintained at 40-50°C.

[0014] Preferably, the slurry in step S4 is provided with a water replenishment system.

[0015] Preferably, in step S7, a saturated steam pressure of 1.2 MPa is passed through the autoclave and heated at 200-210° C. for 7 h.

[0016] Preferably, the lump lime in S2 is first crushed by a crusher, and the lime after crushing by the crusher is ground and sorted by a Raymond mill to sort out lime with a fineness less than or equal to 0.08 mm, and the sorted lime with a fineness less than or equal to 0.08 mm is transported to a lime bin for storage and standby.

[0017] Preferably, in step S4, during the stirring process, the outer wall of the casting and mixing tank is knocked by a pneumatic silo wall knocking hammer, and the pneumatic silo wall knocking hammer knocks the outer wall of the casting and mixing tank once every 5 seconds.

[0018] (III) Beneficial effects

[0019] 1. The present invention develops a production process for producing autoclaved aerated concrete products from bottom slag and desulfurization sludge based on the three requirements of harmless treatment, low carbon and resource utilization, realizes the comprehensive utilization of solid waste, and turns bottom slag and desulfurization sludge into treasure, which not only solves environmental protection problems, but also greatly reduces production costs and brings obvious economic benefits.

[0020] 2. The present invention uses bottom slag as one of the raw materials for preparing autoclaved aerated concrete blocks, because bottom slag contains more glass after water quenching in a high-temperature molten state and has better activity. As a siliceous material in aerated concrete blocks, it can not only reduce the procurement cost of raw materials, but also reduce the amount of cement used in the production process of aerated concrete blocks. According to test results, bottom slag can achieve 100% replacement of fly ash and other siliceous materials to produce qualified aerated concrete block products;

[0021] 3. The present invention uses desulfurized sludge as one of the raw materials for preparing autoclaved aerated concrete blocks, wherein the main component of the desulfurized sludge is desulfurized gypsum, which can replace gypsum as a retarder to reduce production costs;

[0022] 4. In the process of producing aerated concrete blocks in the present invention, the bottom slag and desulfurization sludge solid waste account for a large proportion of the total amount of production raw materials, which can achieve the goal of resource utilization;

[0023] 5. The present invention uses desulfurized sludge as one of the raw materials for preparing autoclaved aerated concrete blocks. Since the chloride ion content in the desulfurized sludge is relatively high, the chloride ion will aggravate the corrosion of steel bars and is not suitable for application in reinforced concrete building materials. However, for autoclaved aerated concrete block products, since there is no steel bar inside, the adverse effects of chloride ions can be avoided;

[0024] 6. The present invention uses desulfurized sludge as one of the raw materials for preparing autoclaved aerated concrete blocks. Since desulfurized sludge may contain a small amount of heavy metals, and since autoclaved aerated concrete block products have the characteristics of high strength, low permeability, high durability, etc., it is suitable as an adhesive for fixing heavy metals to control adverse effects on the environment;

[0025] 7. The present invention uses desulfurized sludge as one of the raw materials for preparing autoclaved aerated concrete blocks. Since desulfurized sludge often contains pathogenic bacteria and other microorganisms, the autoclaved aerated concrete block products contain strong alkalinity during the production process and need to be autoclaved at high temperature to prevent the proliferation of bacteria.

[0026] 8. The present invention uses desulfurized sludge as one of the raw materials for preparing autoclaved aerated concrete blocks. Since the desulfurized sludge has finer particles, it does not need to be ground as raw material, thus reducing power consumption;

[0027] 9. The present invention uses bottom slag and desulfurization sludge as raw materials for preparing autoclaved aerated concrete blocks. Since bottom slag and desulfurization sludge are often strongly alkaline, the slurry (containing calcium hydroxide) used in the production of aerated concrete blocks is highly alkaline, and the alkalinity of solid waste will not affect production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a process flow chart for the production of autoclaved aerated concrete blocks. DETAILED DESCRIPTION

[0029] The following will be combined with the attached embodiment of the present invention Figure 1 The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] S1. Raw material preparation: The raw materials that need to be prepared include bottom slag, desulfurization sludge, cement, lime, aluminum paste, and admixtures.

[0032] S2. Raw material processing: Bottom ash and desulfurization sludge are made into slurry and stored in a slurry tank for standby use. The slurry preparation method is as follows: 1) The bottom ash is piled up in the yard for drainage. After its moisture content is reduced to below 25%, 75 parts by weight of the bottom ash is transported to the ball mill through a grab crane, a slag feed hopper, and a weighing belt conveyor; 2) 3 parts by weight of the desulfurization sludge are transported to the ball mill through a grab crane; 3) 55 parts by weight of the waste slurry is transported to the ball mill, and then the ball mill is started to grind the bottom ash and desulfurization sludge to make slurry. The fineness of the slurry is 20%-25% (80 micron sieve) and the moisture content is 40%. The waste slurry comes from the batching and pouring section and the flipping and cutting section. The waste slurry collected in these two sections is stored in a waste slurry storage tank and transported to the ball mill through a pipeline; 4) The prepared slurry is transported to the slurry tank for storage. The raw material block lime is first crushed by a crusher, and then the crushed lime is ground and sorted by a Raymond mill, and lime with a fineness of less than or equal to 0.08mm is sorted out, and the sorted lime with a fineness of less than or equal to 0.08mm is transported to the lime silo for storage. Cement is stored in the cement silo for use, and 42.5 silicate cement is used for cement. Aluminum paste is stored in an aluminum paste storage tank for use, and admixtures are stored in an admixture storage tank for use, and aluminum paste uses GLS-65.

[0033] S3, Mould oiling section: Apply the release agent evenly on all surfaces inside the mould.

[0034] S4, pouring and batching section: first, add 78 parts by weight of slurry, 8 parts by weight of lime powder and 8 parts by weight of cement into the pouring and mixing tank in sequence, introduce steam into the pouring and mixing tank for heating, so that the temperature in the pouring and mixing tank is maintained at 40-50°C, and then stir for 80 seconds, then add 0.08 parts by weight of aluminum paste into the pouring and mixing tank and stir for 10 seconds, and finally add 0.03 parts by weight of foam stabilizer into the pouring and mixing tank and stir for 120 seconds. During the stirring process, the pneumatic silo wall percussion hammer knocks the outer wall of the pouring and mixing tank once every 5 seconds. During the pouring and mixing process, there will be a shortage of water due to various factors. When the central control system detects a shortage of water, the water replenishment system will start and meter water into the pouring and mixing tank. The water replenishment is industrial water, that is, waste slurry. The waste slurry in the waste slurry storage tank is transported to the pouring mixer through a pipeline.

[0035] S5, static stop pre-curing section: the prepared green body slurry is unloaded into the mold through the pouring discharge port, the discharge temperature is controlled at 43°C, the mold is transported by means of pouring shuttle, static stop room traction machine and other equipment, the green body slurry is transported to the static stop room for pre-curing process, the green body slurry is pre-formed into green body, and after the pre-curing is completed, it is transported to the designated position of the flipping and cutting section, wherein the pre-curing room temperature is 40-50°C, and the static stop time is 2 hours and 45 minutes.

[0036] S6, turning and cutting section: the pre-cured green body and mold are hoisted to the cutting trolley by the turning sling, turned and demoulded, and then cut to size by the longitudinal cutting machine and the transverse cutting machine, and the cutting temperature is 75-95℃;

[0037] S7, autoclave curing section: the cut green bodies and the side plates carrying the green bodies are carried by the autoclave trolley and transported to the autoclave for autoclave curing, and then transported to the section at the designated position of the packaging line. The autoclave is heated at 200-210℃ for 7h under saturated steam pressure of 1.2MPa;

[0038] S8, Palletizing and Packaging Section: Palletize and pack the autoclaved and cured green bodies and transport them to the workshop door for easy handling by forklift.

[0039] Embodiment 2:

[0040] S1. Raw material preparation: The raw materials that need to be prepared include bottom slag, desulfurization sludge, cement, lime, aluminum paste, and admixtures.

[0041] S2. Raw material processing: Bottom ash and desulfurization sludge are made into slurry and stored in a slurry tank for standby use. The slurry preparation method is as follows: 1) The bottom ash is piled up in the yard for drainage. After its moisture content is reduced to below 25%, 76 parts by weight of the bottom ash are transported to the ball mill through a grab crane, a slag feed hopper, and a weighing belt conveyor; 2) 4 parts by weight of the desulfurization sludge are transported to the ball mill through a grab crane; 3) 58 parts by weight of the waste slurry are transported to the ball mill, and then the ball mill is started to grind the bottom ash and desulfurization sludge to make slurry. The fineness of the slurry is 20%-25% (80 micron sieve) and the moisture content is 40%. The waste slurry comes from the batching and pouring section and the flipping and cutting section. The waste slurry collected in these two sections is stored in a waste slurry storage tank and transported to the ball mill through a pipeline; 4) The prepared slurry is transported to the slurry tank for storage. The raw material block lime is first crushed by a crusher, and then the crushed lime is ground and sorted by a Raymond mill, and lime with a fineness of less than or equal to 0.08mm is sorted out, and the sorted lime with a fineness of less than or equal to 0.08mm is transported to the lime silo for storage. Cement is stored in the cement silo for use, and 42.5 silicate cement is used for cement. Aluminum paste is stored in an aluminum paste storage tank for use, and admixtures are stored in an admixture storage tank for use, and aluminum paste uses GLS-65.

[0042] S3, Mould oiling section: Apply the release agent evenly on all surfaces inside the mould.

[0043] S4, pouring and batching section: first, add 79 parts by weight of slurry, 9 parts by weight of lime powder and 9 parts by weight of cement into the pouring and mixing tank in sequence, introduce steam into the pouring and mixing tank for heating, so that the temperature in the pouring and mixing tank is maintained at 40-50°C, and then stir for 83 seconds, then add 0.09 parts by weight of aluminum paste into the pouring and mixing tank and stir for 11 seconds, and finally add 0.04 parts by weight of foam stabilizer into the pouring and mixing tank and stir for 123 seconds. During the stirring process, the pneumatic silo wall percussion hammer knocks the outer wall of the pouring and mixing tank once every 5 seconds. During the pouring and mixing process, there will be a lack of water due to various factors. When the central control system detects a lack of water, the water replenishment system will start and meter water into the pouring and mixing tank. The water replenishment is industrial water, that is, waste slurry. The waste slurry in the waste slurry storage tank is transported to the pouring mixer through a pipeline.

[0044] S5, static pre-curing section: the prepared green body slurry is unloaded into the mold through the pouring discharge port, the discharge temperature is controlled at 43°C, the mold is transported by means of casting shuttle, static room traction machine and other equipment, the green body slurry is transported to the static room for pre-curing process, the green body slurry is pre-formed into green body, and after the pre-curing is completed, it is transported to the designated position of the flipping and cutting section, wherein the pre-curing room temperature is 40-50°C, and the static time is 2 hours and 30 minutes.

[0045] S6, turning and cutting section: the pre-cured green body and mold are hoisted to the cutting trolley by the turning sling, turned and demoulded, and then cut to size by the longitudinal cutting machine and the transverse cutting machine, and the cutting temperature is 75-95℃;

[0046] S7, autoclave curing section: the cut green bodies and the side plates carrying the green bodies are carried by the autoclave trolley and transported to the autoclave for autoclave curing, and then transported to the section at the designated position of the packaging line. The autoclave is heated at 200-210℃ for 7h under saturated steam pressure of 1.2MPa;

[0047] S8, Palletizing and Packaging Section: Palletize and pack the autoclaved and cured green bodies and transport them to the workshop door for easy handling by forklift.

[0048] Embodiment 3:

[0049] S1. Raw material preparation: The raw materials that need to be prepared include bottom slag, desulfurization sludge, cement, lime, aluminum paste, and admixtures.

[0050] S2. Raw material processing: Bottom ash and desulfurization sludge are made into slurry and stored in a slurry tank for standby use. The slurry preparation method is as follows: 1) The bottom ash is piled up in the yard for drainage. After its moisture content is reduced to below 25%, 77 parts by weight of the bottom ash is transported to the ball mill through a grab crane, a slag feed hopper, and a weighing belt conveyor; 2) 5 parts by weight of the desulfurization sludge are transported to the ball mill through a grab crane; 3) 60 parts by weight of the waste slurry is transported to the ball mill, and then the ball mill is started to grind the bottom ash and desulfurization sludge to make slurry. The fineness of the slurry is 20%-25% (80 micron sieve) and the moisture content is 40%. The waste slurry comes from the batching and pouring section and the flipping and cutting section. The waste slurry collected in these two sections is stored in a waste slurry storage tank and transported to the ball mill through a pipeline; 4) The prepared slurry is transported to the slurry tank for storage. The raw material block lime is first crushed by a crusher, and then the crushed lime is ground and sorted by a Raymond mill, and lime with a fineness of less than or equal to 0.08mm is sorted out, and the sorted lime with a fineness of less than or equal to 0.08mm is transported to the lime silo for storage. Cement is stored in the cement silo for use, and 42.5 silicate cement is used for cement. Aluminum paste is stored in an aluminum paste storage tank for use, and admixtures are stored in an admixture storage tank for use, and aluminum paste uses GLS-65.

[0051] S3, Mould oiling section: Apply the release agent evenly on all surfaces inside the mould.

[0052] S4, pouring and batching section: first, add 78.5 parts by weight of slurry, 9.5 parts by weight of lime powder and 9.5 parts by weight of cement into the pouring and mixing tank in sequence, introduce steam into the pouring and mixing tank for heating, so that the temperature in the pouring and mixing tank is maintained at 40-50°C, and then stir for 85 seconds, then add 0.095 parts by weight of aluminum paste into the pouring and mixing tank and stir for 11.5 seconds, and finally add 0.05 parts by weight of foam stabilizer into the pouring and mixing tank and stir for 125 seconds. During the stirring process, the pneumatic silo wall percussion hammer knocks the outer wall of the pouring and mixing tank once every 5 seconds. During the pouring and mixing process, there will be a lack of water due to various factors. When the central control system detects a lack of water, the water replenishment system will start and meter water into the pouring and mixing tank. The water replenishment is industrial water, that is, waste slurry. The waste slurry in the waste slurry storage tank is transported to the pouring mixer through a pipeline.

[0053] S5, static pre-curing section: the prepared green body slurry is unloaded into the mold through the pouring discharge port, the discharge temperature is controlled at 43°C, the mold is transported by means of casting shuttle, static room traction machine and other equipment, the green body slurry is transported to the static room for pre-curing process, the green body slurry is pre-formed into green body, and after the pre-curing is completed, it is transported to the designated position of the flipping and cutting section, wherein the pre-curing room temperature is 40-50°C, and the static time is 2 hours and 15 minutes.

[0054] S6, turning and cutting section: the pre-cured green body and mold are hoisted to the cutting trolley by the turning sling, turned and demoulded, and then cut to size by the longitudinal cutting machine and the transverse cutting machine, and the cutting temperature is 75-95℃;

[0055] S7, autoclave curing section: the cut green bodies and the side plates carrying the green bodies are carried by the autoclave trolley and transported to the autoclave for autoclave curing, and then transported to the section at the designated position of the packaging line. The autoclave is heated at 200-210℃ for 7h under saturated steam pressure of 1.2MPa;

[0056] S8, Palletizing and Packaging Section: Palletize and pack the autoclaved and cured green bodies and transport them to the workshop door for easy handling by forklift.

[0057] Embodiment 4:

[0058] S1. Raw material preparation: The raw materials that need to be prepared include bottom slag, desulfurization sludge, cement, lime, aluminum paste, and admixtures.

[0059] S2. Raw material processing: Bottom ash and desulfurization sludge are made into slurry and stored in a slurry tank for standby use. The slurry preparation method is as follows: 1) The bottom ash is piled up in the yard for drainage. After its moisture content is reduced to below 25%, 80 parts by weight of the bottom ash are transported to the ball mill through a grab crane, a slag feed hopper, and a weighing belt conveyor; 2) 6 parts by weight of the desulfurization sludge are transported to the ball mill through a grab crane; 3) 65 parts by weight of the waste slurry are transported to the ball mill, and then the ball mill is started to grind the bottom ash and desulfurization sludge to make slurry. The fineness of the slurry is 20%-25% (80 micron sieve) and the moisture content is 40%. The waste slurry comes from the batching and pouring section and the flipping and cutting section. The waste slurry collected in these two sections is stored in a waste slurry storage tank and transported to the ball mill through a pipeline; 4) The prepared slurry is transported to the slurry tank for storage. The raw material block lime is first crushed by a crusher, and then the crushed lime is ground and sorted by a Raymond mill, and lime with a fineness of less than or equal to 0.08mm is sorted out, and the sorted lime with a fineness of less than or equal to 0.08mm is transported to the lime silo for storage. Cement is stored in the cement silo for use, and 42.5 silicate cement is used for cement. Aluminum paste is stored in an aluminum paste storage tank for use, and admixtures are stored in an admixture storage tank for use, and aluminum paste uses GLS-65.

[0060] S3, Mould oiling section: Apply the release agent evenly on all surfaces inside the mould.

[0061] S4, pouring and batching section: first, add 80 parts by weight of slurry, 10 parts by weight of lime powder and 10 parts by weight of cement into the pouring and mixing tank in sequence, introduce steam into the pouring and mixing tank for heating, so that the temperature in the pouring and mixing tank is maintained at 40-50°C, and then stir for 90 seconds, then add 0.1 parts by weight of aluminum paste into the pouring and mixing tank and stir for 12 seconds, and finally add 0.06 parts by weight of foam stabilizer into the pouring and mixing tank and stir for 130 seconds. During the stirring process, the pneumatic silo wall percussion hammer knocks the outer wall of the pouring and mixing tank every 5 seconds. During the pouring and mixing process, there will be a lack of water due to various factors. When the central control system detects a lack of water, the water replenishment system will start and meter water into the pouring and mixing tank. The water replenishment is industrial water, that is, waste slurry. The waste slurry in the waste slurry storage tank is transported to the pouring mixer through a pipeline.

[0062] S5, static pre-curing section: the prepared green body slurry is unloaded into the mold through the pouring discharge port, the discharge temperature is controlled at 43°C, the mold is transported by means of casting shuttle, static room traction machine and other equipment, the green body slurry is transported to the static room for pre-curing process, the green body slurry is pre-formed into green body, and after the pre-curing is completed, it is transported to the designated position of the flipping and cutting section, wherein the pre-curing room temperature is 40-50°C, and the static time is 2 hours and 35 minutes.

[0063] S6, turning and cutting section: the pre-cured green body and mold are hoisted to the cutting trolley by the turning sling, turned and demoulded, and then cut to size by the longitudinal cutting machine and the transverse cutting machine, and the cutting temperature is 75-95℃;

[0064] S7, autoclave curing section: the cut green bodies and the side plates carrying the green bodies are carried by the autoclave trolley and transported to the autoclave for autoclave curing, and then transported to the section at the designated position of the packaging line. The autoclave is heated at 200-210℃ for 7h under saturated steam pressure of 1.2MPa;

[0065] S8, Palletizing and Packaging Section: Palletize and pack the autoclaved and cured green bodies and transport them to the workshop door for easy handling by forklift.

[0066] The relevant performance tests are as follows:

[0067] 1. Comparison of chemical composition ranges of fly ash and bottom slag (%)

[0068]

[0069] As can be seen from the above table, the chemical compositions of fly ash and bottom slag are very similar.

[0070] 2. The blocks prepared in Examples 1-4 were tested for appearance quality, strength level, drying shrinkage, frost resistance and thermal conductivity. The test method was based on GB / T 11969-2020 "Test Method for Properties of Autoclaved Aerated Concrete". The test results are as follows:

[0071]

[0072]

[0073] It can be seen that the blocks prepared using bottom slag and desulfurization sludge as raw materials meet the requirements of the national standard GB / T11968-2020 "Autoclaved Aerated Concrete Blocks".

[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants, characterized in that: The steps include: S1. Raw material preparation: The raw materials that need to be prepared include bottom slag, desulfurization sludge, cement, lime, aluminum paste, and admixtures; S2. Raw material processing: the bottom slag and desulfurization sludge are made into slurry and stored in the slurry tank for standby use; the lime is ground into lime powder and stored in the lime silo for standby use; the cement is stored in the cement silo for standby use; the aluminum paste is stored in the aluminum paste storage tank for standby use; and the admixture is stored in the admixture storage tank for standby use; S3, mold oiling section: evenly apply the release agent on all surfaces inside the mold; S4, pouring batching section: add slurry, lime powder, cement, aluminum paste, and admixture into a pouring mixer by conveying and metering, and stir evenly to prepare green body slurry, wherein the proportions are as follows: 78-80 parts of slurry, 8-10 parts of lime powder, 8-10 parts of cement, 0.08-0.1 parts of aluminum paste, and 0.03-0.06 parts of admixture; S5, static stop pre-curing section: the prepared green body slurry is loaded into the mold, and the mold is transported by a casting shuttle, a static stop room tractor and other equipment to transport the green body slurry to the static stop room for pre-curing process, and the green body slurry is pre-formed into a green body, and after the pre-curing is completed, it is transported to the designated position of the flipping and cutting section; S6, turning and cutting section: the pre-cured green body and mold are hoisted to the cutting trolley by the turning sling, turned and demoulded, and then cut to size by the longitudinal cutting machine and the transverse cutting machine; S7, autoclave curing section: the cut green bodies and the side plates carrying the green bodies are carried by the autoclave trolley and transported to the autoclave for autoclave curing, and then transported to the section at the designated position of the packaging line; S8, Palletizing and Packaging Section: Palletize and pack the autoclaved and cured green bodies and transport them to the workshop door for easy handling by forklift.

2. A method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants, characterized in that: The method for preparing slurry from bottom ash and desulfurization sludge in step S2 is as follows: 1) The bottom slag is piled up in the yard to drain water. After its moisture content is reduced to below 25%, it is transported to the ball mill through the grab crane, slag feeding hopper and weighing belt conveyor; 2) Transport the desulfurized sludge to the ball mill through a grab crane; 3) conveying the waste slurry to a ball mill, and then starting the ball mill to grind the bottom ash and desulfurization sludge into slurry, wherein the weight ratio of the bottom ash, desulfurization sludge and waste slurry is: (75-80): (3-6): (55-65); 4) Transport the prepared slurry to the slurry tank for storage.

3. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 2, characterized in that: The waste slurry is circulated and stored in the workshop through the waste slurry circulation section.

4. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 1, characterized in that: The additive is a foam stabilizer.

5. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 4, characterized in that: In step S4, the slurry, lime powder and cement are first added into the pouring mixing tank in sequence and stirred for 80 to 90 seconds, and then the aluminum paste is added and stirred for 10 to 12 seconds, and then the foam stabilizer is added and stirred for another 120 to 130 seconds.

6. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 1, characterized in that: During step S4, steam is introduced into the pouring and mixing tank for heating, so that the temperature in the pouring and mixing tank is maintained at 40-50°C.

7. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 2, characterized in that: The slurry in step S4 is provided with a water replenishment system.

8. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 1, characterized in that: In step S7, a saturated vapor pressure of 1.2 MPa is passed through the autoclave and heated at 200-210° C. for 7 h.

9. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 1, characterized in that: The lump lime in S2 is firstly crushed by a crusher, and the crushed lime is ground and sorted by a Raymond mill to sort out the lime with a fineness less than or equal to 0.08 mm, and the sorted lime with a fineness less than or equal to 0.08 mm is transported to a lime silo for storage and standby use.

10. The method for preparing autoclaved aerated concrete blocks using bottom ash and desulfurized sludge from coal-fired power plants according to claim 1, characterized in that: In step S4, during the mixing process, the outer wall of the pouring and mixing tank is knocked by a pneumatic silo wall knocking hammer, and the pneumatic silo wall knocking hammer knocks the outer wall of the pouring and mixing tank once every 5 seconds.

Citation Information

Patent Citations

  • Manufacture method for autoclaved fly-ash aerated concrete block

    CN105130324A

  • Flyash-sand autoclaved aerated concrete block and preparation method thereof