High-solid-content nano aluminum oxide ceramic feed and feed injection molding method

Through the feeding formula of nano alumina ceramics with high solid content and the composite extraction solvent system, the problem that nano alumina powder is difficult to obtain high-density ceramic injection products is solved, and the sintering density and density of high-density alumina ceramics are achieved. promote.

CN118955097APending Publication Date: 2024-11-15苏州芯合半导体材料有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410944945.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, it is difficult to obtain high-density alumina ceramic injection products using nano-scale alumina powders, mainly due to excessive addition of organic matter, resulting in a decrease in density and sintering deformation.

Method used

Using a high solids content nano-alumina ceramic feeding formula, including alumina powders, microcrystalline wax, beeswax, polyvinyl butyral, polyvinyl alcohol PEG6000, high density polyethylene, stearic acid and oleic acid, through Compound surfactant system and compound extraction solvent system to increase solid content and reduce the risk of defects during degreasing.

Benefits of technology

High-density injection molding of nano-alumina ceramic feed was achieved, and the ceramic sintering density reached 3.96g/cm3, which reduced the amount of binder and reduced sintering deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure FDA0004945353680000011
    Figure FDA0004945353680000011
  • Figure FDA0004945353680000012
    Figure FDA0004945353680000012
Patent Text Reader

Abstract

The invention relates to the field of ceramic powder injection molding, in particular to a high-solid-content nanometer aluminum oxide ceramic feed and a feed injection molding method. The preparation method comprises the following steps: uniformly mixing polyvinyl alcohol of a water-soluble system and microcrystalline wax and beeswax of an oil removal system through a composite surface active system consisting of stearic acid, oleic acid and dibutyl phthalate, and then dissolving and removing various components at one time through a compound solvent consisting of n-heptane, alcohol and pure water, thereby obtaining the sintered compact high-solid-content and high-oil-removal-rate wax with high solid content. And the alumina product is not easy to crack. According to the high-solid-content nanometer aluminum oxide ceramic feed, the proportion of nanometer aluminum oxide reaches up to 88 wt%-89 wt%, the adding amount of other organic matter is only 11 wt%-15 wt%, and the ceramic sintering density of an obtained high-density aluminum oxide ceramic injection product reaches up to 3.96%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic powder injection molding, in particular to a nano-alumina ceramic feed with a high solid content and a feed injection molding method. Background Art

[0002] Injection molding feed binder systems are mainly divided into three categories according to different degreasing methods, direct thermal degreasing, solvent degreasing and catalytic degreasing. The feed binder formulas for direct thermal degreasing and catalytic degreasing usually contain more resin-based binder materials. When the particle size of ceramic powder is nanometer level, due to the high specific surface area of ​​the powder, the resin-based feed formula system needs to reduce the solid content and add more organic matter to ensure the fluidity of the feed. The solvent degreasing feed formula system usually adopts a two-step degreasing method of solvent extraction and heating degreasing. First, most of the organic matter is removed by solvent, and then thermal degreasing is performed to remove the remaining polymer resin.

[0003] When the particle size D50 of the ceramic powder is about 400 nanometers, it is usually necessary to add 15-25% by mass of organic matter to ensure the fluidity of the feed. For example, in the Chinese invention patent application with publication number CN 113213896 A, "A feed for aluminum oxide ceramic injection molding and a feed injection molding method", a feed formula is disclosed, which uses 70wt%-85wt% of aluminum oxide powder of French Arteo model P172LSB and 15wt%-30wt% of organic matter. The density of the final product is 3.93g / cm 3 , its organic matter content is still relatively high.

[0004] However, adding too much organic matter will lead to a decrease in the density of the sintered ceramics and easily cause sintering deformation, so it is difficult to obtain high-density alumina ceramic injection products. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the defect in the prior art that it is difficult to obtain high-density alumina ceramic injection products when nano-scale alumina powder is used to prepare alumina ceramic injection products, and to provide a high-solid content nano alumina ceramic feeding and feeding injection molding method.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A high solid content nano-alumina ceramic feedstock comprises the following components in weight percentage:

[0008] Alumina powder 87%-89%;

[0009] Microcrystalline wax 3.3%-3.9%

[0010] Beeswax 2.75%-3.25%

[0011] Polyvinyl butyral 1.1%-1.3%

[0012] Polyvinyl alcohol PEG6000 0.55%-0.65%

[0013] High density polyethylene 1.65%-1.95%

[0014] Stearic acid 0.64%-0.76%

[0015] Oleic acid 0.55%-0.65%

[0016] Dibutyl phthalate 0.46%-0.54%

[0017] The sum of the weight percentages of the various components is 100%.

[0018] Polyvinyl alcohol is a water-soluble system, microcrystalline wax and beeswax are oil-removing systems. The present invention mixes the two systems evenly through a composite surfactant system composed of stearic acid, oleic acid and dibutyl phthalate, and increases the solid content of the feed on the basis of ensuring the fluidity of the injection feed, and the alumina powder is as high as 88wt%-89wt%; in order to prevent cracking, swelling and other defects caused by increased solid content and reduced organic matter content during the degreasing process, a composite extraction solvent system of n-heptane+alcohol+pure water is used for degreasing treatment, microcrystalline wax and beeswax are easily soluble in n-heptane, and polyvinyl alcohol is easily soluble in water. Most of the organic matter is removed by the composite extraction solvent, providing a channel for the removal of long-chain polymers such as high-density polyethylene, thereby reducing the risk of cracking of the product during the degreasing process and obtaining a high-density alumina ceramic injection product.

[0019] A feeding injection molding method for a high-solid content nano-alumina ceramic feedstock comprises the following steps:

[0020] First, the above-mentioned alumina powder and various organic mixed materials are added into an internal mixer in proportion and mixed. After mixing, the feed is made into feed particles by a granulator.

[0021] Put the feed particles into the hopper of the injection machine, the screw temperature is up to 165℃, and the injection product blank is obtained by injection;

[0022] The blank of the injection product is placed in a compound solvent, the compound solvent formula is: 60wt% n-heptane, 30wt% alcohol and 10wt% pure water; after heating the compound solvent, a circulating pump and a stirring paddle are used in the solvent extraction tank to mix the liquid evenly and fully flow, and the extraction time is about 8 hours. After completion, the blank is placed in an oven for drying. The dried blank is placed in a degreasing furnace for heating and degreasing, and the degreased blank is placed in a high-temperature sintering furnace for sintering to obtain a sintered dense alumina product.

[0023] The beneficial effects achieved by the present invention are as follows: the proportion of nano-alumina in the high-solid content nano-alumina ceramic feed of the present invention is as high as 88wt%-89wt%, and the addition amount of the remaining organic matter is only 11wt%-15wt%. Through the action of the composite surfactant system, the amount of binder is reduced, and the ceramic sintering density of the obtained high-density alumina ceramic injection product is as high as 3.96%. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0025] Example

[0026] A feeding injection molding method for a high-solid content nano-alumina ceramic feedstock comprises the following steps:

[0027] First, heat the mixer to 120℃ and add alumina powder with a D50 of 400 nanometers. After 10 minutes, raise the mixer temperature to 160℃, set the rotor speed to 35 rpm and push the top hammer down. Add half the weight of the powder first, mix for five minutes, then add all the additives, push the top hammer down and mix for 5 minutes, and finally add all the remaining powder.

[0028] After mixing for 15 minutes, the temperature was lowered to 150°C and mixed for 1.5 hours. After the internal mixing, the feed was passed through a granulator to form 2 mm feed particles.

[0029] Put the feed particles into the hopper of the injection machine, the screw temperature is up to 165℃, the injection pressure is 60Mpa, the injection speed is 35mm / s, the holding pressure is 40Mpa, and the holding time is 2s to obtain the injection product blank;

[0030] Place the injection product blank in the solvent, heat the solvent to 43°C, and use a circulating pump and a stirring paddle in the solvent extraction tank to mix the liquid evenly and make it flow fully. The extraction time is 8 hours. After completion, place the blank in a 50°C oven for drying. The compound solvent formula is: 60% Wt of n-heptane, 30% Wt of alcohol, and 10 Wt of pure water. Comparative Examples 1-3 are degreased by n-heptane degreasing, n-heptane + pure water degreasing, or direct thermal degreasing.

[0031] The dried blank is placed in a degreasing furnace and heated to 600°C for 28 hours, and kept at this temperature for 2 hours;

[0032] The degreased blank was placed in a high-temperature sintering furnace, and the temperature was raised to 1580°C at a rate of 10°C / min and kept at that temperature for 2 hours to obtain a sintered dense alumina product.

[0033] Table 1 Component ratio of each embodiment

[0034]

[0035]

[0036] Note: The contents of the components in Table 1 are in weight percentage. The purity of alumina of Sumitomo AES-11C is 99.9% and the particle size D50 is 430 nm.

[0037] It can be seen that the present invention uses the surfactant effect of stearic acid, oleic acid and dibutyl phthalate to evenly mix the water-soluble system of polyvinyl alcohol and the oil-removing system of microcrystalline wax and beeswax, and then uses a solvent composed of n-heptane-alcohol-pure water to dissolve and remove multiple components at one time, thereby obtaining a sintered, dense, high-solid content, and non-cracking alumina product.

[0038] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high solid content nano alumina ceramic feed, It is characterized in that It is composed of the following components in percentage by weight:

2. The high solid content nano-alumina ceramic feed material as claimed in claim 1, It is characterized in that The composition comprises the following components in weight percentage:

3. The high solid content nano alumina ceramic feed material as claimed in claim 1 or 2, It is characterized in that The grade of the alumina powder is Japan Sumitomo AES-11C.

4. The feeding injection molding method of the high solid content nano-alumina ceramic feedstock according to claim 1, It is characterized in that After the injection product blank is obtained, the injection product blank is placed in a compound solvent for degreasing, wherein the compound solvent consists of 60wt% of n-heptane, 30wt% of alcohol and 10wt% of pure water.

Citation Information

Patent Citations

  • Method for manufacturing dentate special-shaped ceramic components by injection molding

    CN101643360A

  • Preparation and application methods of thermoplastic adhesive for powder microinjection molding

    CN102775673A

  • Defect visualization analysis method for preparing turbine through powder injection molding and preparation method of titanium-aluminum alloy turbine

    CN112632716A

  • Preparation method of high-toughness aluminum oxide ceramic

    CN114478041A

  • Alumina feed as well as preparation method and application thereof

    CN116102341A