Indium tin oxide target material and preparation method and application thereof

By doping SnO2, ZnO and B2O3 in the indium tin oxide target, glass powder is formed to reduce the sintering temperature and refine the grains, the problem of "nodonation" phenomenon of indium tin oxide target during coating is solved, and the problem of "nodonation" of indium tin oxide target is improved Target density and coating quality.

CN118955118APending Publication Date: 2024-11-15ZHONGSHAN ZL ADVANCED MATERIALS TECHNOLOGY

Patent Information

Application Number
CN202411023847.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Indium tin oxide targets are prone to "nodonation" during physical vapor deposition coating, which affects service life and the quality of transparent oxide films.

Method used

By doping SnO2, ZnO and B2O3 as glass powder into In2O3, using B2O3 as glass network forming agent and ZnO as glass stabilizer, the sintering temperature is reduced and the grains are refined, the target density is improved, and the noduling is improved. "Phenomenon.

Benefits of technology

It significantly reduces the sintering temperature and grain size, improves the density of the target material, improves the "nodonation" phenomenon, and improves the coating quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968007880000041
    Figure BDA0004968007880000041
  • Figure BDA0004968007880000042
    Figure BDA0004968007880000042
Patent Text Reader

Abstract

The invention discloses an indium tin oxide target material as well as a preparation method and application thereof. The invention provides an indium tin oxide target material. The indium tin oxide target material comprises the following raw materials: In2O3 and glass powder, the glass powder is prepared from the following components: SnO2, ZnO and B2O3. According to the invention, B2O3 is selected as a glass network forming agent, a glass state stabilizer of ZnO and SnO2 are selected as a base material of glass, and various oxides are doped into In2O3 in the form of glass powder, so that the sintering temperature can be obviously reduced, the grain size can be refined, and the compactness of the target material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal target materials, and in particular to an indium tin oxide target material and a preparation method and application thereof. Background Art

[0002] Transparent conducting oxides (TCO) films prepared by physical vapor deposition (PVD) technology using indium tin oxide (ITO) targets as the main raw material have excellent conductivity and light transmittance, and are therefore widely used in display, solar cells, electrochromic and other fields. However, ITO targets often show "nodule" during the PVD coating process, which has a significant impact on the service life of the targets and the quality of TCO films.

[0003] Therefore, it is necessary to provide a new indium tin oxide target. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides an indium tin oxide target material, which can effectively reduce the sintering temperature of the target material and refine the grains.

[0005] The second aspect of the present invention also provides a method for preparing an indium tin oxide target.

[0006] The third aspect of the present invention also provides an application of an indium tin oxide target.

[0007] An indium tin oxide target material provided according to an embodiment of the first aspect of the present invention includes the following raw materials: In2O3 and glass powder; the components of the glass powder include SnO2, ZnO and B2O3.

[0008] The indium tin oxide target according to the embodiment of the present invention has at least the following beneficial effects:

[0009] The present invention selects B2O3 as a glass network former, ZnO as a glass stabilizer, and SnO2 as a glass matrix material, and dopes it into In2O3 in the form of glass powder, which can significantly reduce the sintering temperature and refine the grain size, thereby improving the density of the target material. By improving the density of the target material, the "nodule" phenomenon is significantly improved; this is because glass has a lower softening temperature and melting point, softens at a lower temperature, and exhibits good wetting behavior on the ceramic matrix, which enables the ceramic particles to better contact and bond during the sintering process, allowing the liquid phase to appear at a lower temperature, thereby promoting sintering.

[0010] According to some embodiments of the present invention, based on the total mass of the indium tin oxide target material, the glass powder accounts for 1% to 10% of the total mass.

[0011] According to some embodiments of the present invention, the glass powder accounts for 3% to 10% of the total mass of the indium tin oxide target. Further includes the numerical values ​​and subset ranges between 3% and 10%. For example, it includes 3%, 5%, 7%, 10% or a range consisting of any two numerical values. Therefore, within the above range, it has a higher target density and a low sintering temperature.

[0012] The indium tin oxide target material includes the following raw materials calculated by mass percentage:

[0013] In2O3 is 90% to 99%; SnO2 is 0.815% to 9.32%; ZnO is 0.032% to 0.64%; B2O3 is 0.036% to 1.21%; the sum of the mass percentages of each raw material is 100%.

[0014] According to some embodiments of the present invention, the glass powder has a D 50 Particle size ≤1μm.

[0015] According to some embodiments of the present invention, the glass powder is prepared by the following method:

[0016] (1) SnO2, ZnO, B2O3, water and a dispersant are mixed and ball-milled, and dried; then the mixture is ground and sieved to obtain a mixed powder;

[0017] (2) Melting and quenching the sieved mixed powder; adding water and a dispersant to perform ball milling, drying, and grinding to obtain the product.

[0018] According to some embodiments of the present invention, in step (1), the ball milling time is 2 to 6 hours.

[0019] According to some embodiments of the present invention, in step (1), the drying time is 10 to 20 hours.

[0020] According to some embodiments of the present invention, in step (2), the melting temperature is 1500-1650°C.

[0021] According to some embodiments of the present invention, in step (2), the melting time is 2 to 5 hours.

[0022] According to some embodiments of the present invention, in step (2), the ball milling time is 8 to 15 hours.

[0023] According to the second aspect of the present invention, the method for preparing the indium tin oxide target provided by the embodiment comprises the following steps:

[0024] S1. In2O3, glass powder, water and dispersant are mixed and ball-milled; a binder and a plasticizer are added, and a powder is obtained by spray granulation;

[0025] S2, molding the powder and cold isostatically pressing it to obtain a green target;

[0026] S3, degreasing and sintering the green target material.

[0027] According to some embodiments of the present invention, the compression molding pressure is 150 MPa to 220 MPa.

[0028] According to some embodiments of the present invention, the maximum sintering temperature is 1300-1400°C.

[0029] According to some embodiments of the present invention, the sintering step includes: sequentially performing a first sintering, a second sintering and a third sintering.

[0030] According to some embodiments of the present invention, the first sintering temperature is 600-800°C.

[0031] According to some embodiments of the present invention, the temperature of the second sintering is 900-980°C.

[0032] According to some embodiments of the present invention, the temperature of the third sintering is 1300-1400°C.

[0033] According to some embodiments of the present invention, the adhesive comprises PVA.

[0034] According to some embodiments of the invention, the plasticizer comprises PEG.

[0035] According to some embodiments of the present invention, the sintering is performed in an oxygen atmosphere.

[0036] A third aspect of the present invention provides an application of the indium tin oxide target in the field of PVD coating.

[0037] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION

[0038] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0039] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0040] Some of the raw materials used in the present invention are as follows:

[0041] In2O3 powder: particle size 2.0μm<D50<5.0μm, purity 4N and above; commercially available;

[0042] SnO2, ZnO and B2O3: purity is 4N or above; commercially available.

[0043] Example 1

[0044] This example provides an indium tin oxide target material, the component dosage of which is shown in Table 1, and the preparation method thereof is as follows:

[0045] Preparation of glass powder:

[0046] (1) SnO2, ZnO, B2O3, deionized water, zirconium oxide beads and dispersant polyvinyl pyrrolidone are mixed and ball-milled for 2 to 6 hours, and dried; dried in an oven at 150° C. for 15 hours until the water is completely removed; then ground and sieved to obtain a mixed powder;

[0047] (2) The sieved mixed powder was added to a 1550°C frit furnace for melting for 2 h, then quickly poured into deionized water for quenching, deionized water, zirconium oxide beads and dispersant PVP were added for ball milling for 10 h, and dried in an oven at 150°C for 15 h. After grinding and sieving, D 50 Glass powder <1.0μm.

[0048] Preparation of Indium Tin Oxide Target:

[0049] S1. In2O3, glass powder, deionized water and dispersant PVP were mixed and ball-milled for 16 hours to obtain a slurry with a powder particle size of D 50 <0.5μm; adding binder (PVA) and plasticizer (PEG), the binder mass ratio is 1.2%, the plasticizer mass ratio is 0.8%, and the granulated powder is obtained after spray granulation;

[0050] S2, the powder is molded at a pressure of 200 MPa, and a green target is obtained after cold isostatic pressing;

[0051] S3, after degreasing the green target, sinter at high temperature in oxygen atmosphere, the highest sintering temperature is 1400℃, and the total sintering time is 130h. The first stage sintering temperature is 600℃, and the holding time is 3h; the second stage sintering temperature is 900℃, and the holding time is 5h; the third stage sintering temperature is 1400℃, oxygen is introduced, the holding time is 8h, the oxygen introduction rate is 36L / min, and the pressure is 2.3kg / cm 2 .

[0052] Embodiments 2 to 5

[0053] Examples 2 to 5 provide an indium tin oxide target material, and the preparation method thereof is basically the same as that of Example 1, except that the components are used in amounts, which are shown in Table 1.

[0054] Table 1 Examples 1 to 5 (wt.%)

[0055]

[0056] Embodiments 6 to 10

[0057] Examples 6 to 10 provide an indium tin oxide target material, and the preparation method thereof is basically the same as that of Example 1, except that the components are used in amounts, which are shown in Table 2.

[0058] Table 2 Examples 6 to 10 (wt.%)

[0059]

[0060] Comparative Example 1

[0061] Comparative Example 1 uses the same raw material ratio as Example 5, the difference being that, in Comparative Example 1, glass powder is not prepared first, but the raw materials are directly mixed and ball-milled. The other steps are the same as Example 5.

[0062] Comparative Example 2

[0063] Comparative Example 2 uses the same raw material ratio and preparation method as Example 5, the difference being that the raw material of the glass powder does not contain ZnO, and an equal amount of SnO2 is used to replace ZnO.

[0064] Comparative Example 3

[0065] Comparative Example 3 uses the same raw material ratio and preparation method as Example 5, the difference being that the raw material of the glass powder does not contain B2O3, and an equal amount of SnO2 is used to replace B2O3.

[0066] Performance Testing

[0067] The indium tin oxide targets prepared in Examples 1 to 10 of the present invention and Comparative Examples 1 to 3 were tested as follows. The results are shown in Table 3:

[0068] Average grain size: the average grain size measured by the intercept method;

[0069] Relative density: The density of the target material is tested by the Archimedes drainage method.

[0070] Table 3

[0071] Maximum sintering temperature ℃ Average grain size (μm) Relative density (%) Example 1 1400 5.36 98.5 Example 2 1380 5.13 98.9 Example 3 1370 5.03 99.0 Example 4 1360 4.92 99.3 Example 5 1350 4.76 99.7 Example 6 1350 4.53 99.4 Example 7 1340 4.39 99.5 Example 8 1330 4.26 99.5 Example 9 1320 4.08 99.8 Example 10 1300 3.91 99.7 Comparative Example 1 1350 4.98 90.3 Comparative Example 2 1420 5.03 98.1 Comparative Example 3 1470 5.32 98.5

[0072] It can be seen from the experimental data in Table 3 that the indium tin oxide target prepared in Examples 1-10 of the present invention has a sintering temperature of 1300-1400°C, a density of 98.5-99.8%, and an average grain size of 3.91-5.36μm, indicating that this patent prepares the dopant into glass and mixes it with In2O3 in the form of glass powder, which can achieve a low temperature sintering temperature while introducing lower impurities, and obtain a target with high density and lower grain size.

[0073] The raw material ratio and preparation process of Comparative Example 1 and Example 5 are exactly the same, the difference is that Comparative Example 1 is directly mixed, while Example 5 first prepares the dopant into glass and then mixes it. As shown in Table 3, under the same sintering process, the density of Comparative Example 1 is only 90.3%, which is much lower than 99.7% of Example 5, and the grain size of Comparative Example 1 is also larger. This is because SnO 2- ZnO-B2O3 glass has a lower softening temperature and melting point, softens at a lower temperature, and exhibits good wetting behavior on the ceramic matrix, which enables the ceramic particles to better contact and bond during the sintering process. It appears in liquid phase at a lower temperature, promotes sintering densification, and inhibits grain growth to a certain extent.

[0074] The glass powder addition content of Comparative Examples 2 and 3 is the same as that of Example 5, and the difference lies in the difference in the chemical composition of the glass powder. As shown in Table 3, compared with Example 5, the sintering temperatures of Comparative Examples 2 and 3 are 70°C and 120°C higher, respectively, but their densities are lower than those of Example 5. This is because the composition of the glass has a greater influence on its softening temperature, liquid phase viscosity and sintering effect. Therefore, the indium tin oxide target provided by the present invention can significantly reduce the sintering temperature and refine the grain size, thereby improving the density of the target.

[0075] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. An indium tin oxide target, characterized in that: The invention comprises the following raw materials: In2O3 and glass powder; the components of the glass powder include SnO2, ZnO and B2O3.

2. The indium tin oxide target according to claim 1, characterized in that: Calculated based on the total mass of the indium tin oxide target material, the glass powder accounts for 1% to 10% of the total mass.

3. The indium tin oxide target according to claim 1 or 2, characterized in that: The indium tin oxide target material includes the following raw materials calculated by mass percentage: In2O3 is 90% to 99%; SnO2 is 0.815% to 9.32%; ZnO is 0.032% to 0.64%; B2O3 is 0.036% to 1.21%, and the sum of the mass percentages of each raw material is 100%.

4. The indium tin oxide target according to claim 1, characterized in that: The glass powder D 50 Particle size ≤1μm.

5. The indium tin oxide target according to claim 1, characterized in that: The glass powder is prepared by the following method: (1) SnO2, ZnO, B2O3, water and a dispersant are mixed and ball-milled, and dried; then the mixture is ground and sieved to obtain a mixed powder; (2) Melting and quenching the sieved mixed powder; adding water and a dispersant to perform ball milling, drying, and grinding to obtain the product.

6. The method for preparing an indium tin oxide target according to any one of claims 1 to 5, characterized in that: The steps include: S1. In2O3, glass powder, water and dispersant are mixed and ball-milled; a binder and a plasticizer are added, and a powder is obtained by spray granulation; S2, molding the powder and cold isostatically pressing it to obtain a green target; S3, degreasing and sintering the green target material.

7. The preparation method according to claim 6, characterized in that: The compression molding pressure is 150 MPa to 220 MPa.

8. The preparation method according to claim 6, characterized in that: The maximum sintering temperature is 1300-1400°C.

9. The preparation method according to claim 6, characterized in that: The sintering step comprises: sequentially performing a first sintering, a second sintering and a third sintering; Preferably, the first sintering temperature is 600-800°C; Preferably, the second sintering temperature is 900-980°C; Preferably, the temperature of the third sintering is 1300-1400°C.

10. Use of the indium tin oxide target according to any one of claims 1 to 5 in the field of PVD coating.

Citation Information

Patent Citations

  • IZO target and manufacturing method thereof

    CN109837512A

  • Indium zinc tin oxide sputtering target material and conductive film thereof

    CN114574820A

  • Method for producing tin-doped indium oxide particulate

    JP2005035882A

  • The manufacturing methods of target with high density and conductibility by using doped-zinc oxide and doped-tin oxide in indium -zinc -tin oxide system

    KR1020110035239A

Cited By

  • Metal oxide semiconductor target material, preparation method thereof and thin film transistor

    CN119683992A

  • A metal oxide semiconductor target, a preparation method thereof, and a thin film transistor