Photocatalytic porous concrete and test method thereof
By optimizing the porosity of porous concrete and the spraying amount of nano-TiO2 dispersion, combined with photocatalytic technology, the problem of poor microbial killing effect of porous concrete in sewage is solved, and the efficiency of sewage treatment is significantly improved.
Patent Information
- Application Number
- CN202411036761.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Existing porous concrete cannot effectively kill microorganisms in sewage, and the porosity, dispersion concentration and spraying amount have a great impact on the photocatalytic effect, resulting in poor sewage treatment effect.
By preparing porous concrete with a porosity of 6%-10%, nano-TiO2 dispersion was sprayed on the surface, using specific gelling material ratio and spraying amount, combined with ultraviolet light catalysis, the sewage degradation efficiency was optimized.
It has achieved efficient degradation of nitrogen, phosphorus and chemical oxygen demand in sewage, determined the optimal porosity, dispersion concentration and spraying amount, significantly improving the sewage treatment effect of photocatalytic porous concrete.
Smart Images

Figure CN118955174A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of agricultural sewage treatment. Background Art
[0002] Agricultural drainage refers to sewage and liquid waste discharged from crop cultivation, livestock breeding, food processing and other processes in agricultural production. Currently, porous concrete is often used to adsorb pollutants in sewage discharged from farmland drainage. However, porous concrete cannot kill microorganisms in pollutants, so TiO2 photocatalytic dispersion is sprayed on the surface of porous concrete. However, the porosity of porous concrete, the concentration of dispersion and the amount of spraying all affect the sewage treatment effect of photocatalytic porous concrete. Summary of the invention
[0003] In order to obtain the best porosity of porous concrete, concentration of dispersion liquid and spraying amount, the present invention provides a test method for photocatalytic porous concrete.
[0004] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0005] A photocatalytic porous concrete, the surface of which is sprayed with nano-TiO2 dispersion.
[0006] The porosity of the porous concrete is 6%-10%. The materials of the porous concrete include coarse aggregate, fine aggregate, cementitious material and water, and the ratio of coarse aggregate: fine aggregate: cementitious material: water is (12-15): (1.3-1.6): 3.3: 1.
[0007] The cementitious material comprises cement, silica fume, water reducing agent and air entraining agent, wherein the silica fume content is 8% of the total cementitious material, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, the water reducing agent parameter is 1% of the total cementitious material, and the air entraining content is 0.1% of the total cementitious material.
[0008] The spraying amount of the nano-TiO2 dispersion is 200-500g / m 2 , the concentration of nano-TiO2 dispersion is 8%-12%.
[0009] A test method for photocatalytic porous concrete comprises the following steps:
[0010] S1. pouring porous concrete with the same porosity;
[0011] S2 configuration of different concentrations of nano-TiO2 dispersion, and each concentration of nano-TiO2 dispersion were sprayed evenly on each porous concrete to obtain a photocatalytic porous concrete;
[0012] S3. Install a UV light source in the water container and configure a certain concentration of wastewater to be degraded in the water container;
[0013] S4. placing each porous concrete in the wastewater to be degraded;
[0014] S5. After the photocatalytic reaction is completed, the nitrogen, phosphorus and chemical oxygen demand in the degraded wastewater are measured, and the photocatalytic degradation efficiency of the photocatalytic porous concrete sprayed with different concentrations of nano-TiO2 dispersion is calculated based on the measurement results;
[0015] S6. The optimal concentration of nano-TiO2 dispersion is obtained according to the photocatalytic degradation efficiency;
[0016] S7 configure the optimal concentration of nano-TiO2 dispersion, and the dispersion was sprayed on each porous concrete in different spraying amounts;
[0017] S8. Repeat step S5 to obtain the optimal spraying amount of nano-TiO2 dispersion;
[0018] S9. Pouring porous concrete of different porosities, configuring the optimal concentration of nano-TiO2 dispersion, and spraying the dispersion on each porous concrete at the optimal spraying amount;
[0019] S10. Repeat step S5 to obtain the optimal porosity of the porous concrete.
[0020] The step S1 of pouring porous concrete with the same porosity comprises the following steps:
[0021] S1-1. The mixed concrete material is loaded into the mold so that each layer of concrete material has the same thickness. Each layer is loaded with a tamping rod from the edge to the center of the spiral tamping. When the bottom layer of concrete material is tamped, the tamping rod touches the bottom of the mold. When each layer is tamped, the tamping rod is inserted into the next layer of concrete material;
[0022] S1-2. Use a vibrating table to vibrate the concrete material after tamping;
[0023] S1-3. After the vibration is completed, the excess concrete material is removed and smoothed to complete the pouring of the porous concrete in the mold;
[0024] S1-4. After the porous concrete is cast, it is covered with a plastic film and placed in a standard curing room at a temperature of (20±2)°C and a relative humidity of 95% for curing;
[0025] S1-5. De-mould after standing in a standard curing room for 48 hours.
[0026] The step S2 of preparing a nano-TiO2 dispersion and spraying it on the porous concrete comprises the following steps:
[0027] S2-1. Stir the nano-TiO2 powder with water until dissolved;
[0028] S2-2 using a high shear emulsifier to disperse the solution, and then dispersed using an ultrasonic cleaner to obtain a nano-TiO2 dispersion;
[0029] S2-3. Spray the nano-TiO2 dispersion on the porous concrete, let it air dry for 24 hours, and then put it in the curing room for standard curing until 28 days.
[0030] The ultraviolet irradiance of the ultraviolet light source in step S3 is (15±0.5) W / m 2 .
[0031] The step S5 of measuring nitrogen, phosphorus and chemical oxygen demand in the degradation wastewater comprises the following steps:
[0032] S5-1. Use a pipette to collect water from the upper surface of the photocatalytic porous concrete in the water container. Take water samples three times at the diagonal and center points in each time period;
[0033] S5-2. Put the three water samples into polyethylene bottles respectively;
[0034] S5-3. Each water sample was tested three times, and the average of the three tests was taken as the final test result;
[0035] The total nitrogen (TN) content in the degradation wastewater is determined by the following steps:
[0036] S5-3-1-1. Prepare alkaline potassium persulfate solution and hydrochloric acid dilution used for testing nitrogen content;
[0037] S5-3-1-2. Use a pipette to take 5 mL of the water sample to be tested and inject it into a closed digestion tube. Add 5 mL of pure water to the blank group;
[0038] S5-3-1-3. Add 5 mL of alkaline potassium persulfate solution to each test tube, tighten the digestion tube cap, and shake the liquid in the digestion tube thoroughly;
[0039] S5-3-1-4. Turn on the multi-parameter digestion instrument, select TN digestion, heat the machine to 122°C, then put the digestion tube into the digestion tube and digest for 40 minutes;
[0040] S5-3-1-5. After digestion is completed, wait for the test tube to cool down slightly, take it out and place it on the test tube rack, and then put it into the cooling tank to cool;
[0041] S5-3-1-6. After cooling the test tubes to room temperature, add 1 mL of hydrochloric acid diluent, cover the test tubes tightly and shake well;
[0042] S5-3-1-7. Preheat the total nitrogen analyzer and select the sample for measurement; rinse the 10mm cuvette with pure water, pour the blank water sample into the cuvette first, put it into the measuring instrument, and press the blank key to reset to zero after the reading stabilizes;
[0043] S5-3-1-8. Test each water sample in turn, and rinse the cuvette with pure water before testing each water sample. The reading displayed when the cuvette is placed in the measuring instrument is the test result;
[0044] The total phosphorus TP content in the degradation wastewater is determined by the following steps:
[0045] S5-3-2-1. Prepare potassium persulfate, ammonium molybdate and ascorbic acid solution required for testing TP content;
[0046] S5-3-2-2. Use a pipette to take 8 mL of the water sample to be tested and inject it into a closed digestion tube. Add 8 mL of pure water to the blank group.
[0047] S5-3-2-3. After taking the water sample, add 1 mL of potassium persulfate solution to each digestion tube, cover the lid tightly, and shake the solution in the tube thoroughly;
[0048] S5-3-2-4. Select TP digestion on the multi-parameter digestion instrument startup page. After the machine heats up to 120°C, put the digestion tube in and start digestion.
[0049] S5-3-2-5. After digestion for 30 minutes, take out the test tube after it cools down, place it on a test tube rack and put it in a cooling tank to cool to room temperature;
[0050] S5-3-2-6. Take out the test tubes that have been digested and cooled to room temperature, add 1 mL of ascorbic acid solution and 1 mL of ammonium molybdate solution to each test tube, cover the test tubes tightly, shake well, and let stand for color development;
[0051] S5-3-2-7. Preheat the multi-parameter water quality analyzer, select the corresponding test item, first use pure water to rinse the 30mm cuvette, then pour the blank water sample into the cuvette, put it into the measuring instrument, and press the blank key to reset to zero after the reading stabilizes;
[0052] S5-3-2-8. After the instrument is set to zero, each sample to be tested is placed in turn, and the number displayed on the instrument is the test result;
[0053] The determination of the chemical oxygen demand (COD) content in the degradation wastewater includes the following steps:
[0054] S5-3-3-1. Use LH-D and LH-E powders to prepare LH-D reagent and LH-E reagent required for determining COD content;
[0055] S5-3-3-2. Take 2.5 mL of the water sample to be tested and inject it into an open digestion tube. Add 8 mL of pure water to the blank group.
[0056] S5-3-3-3. Add 0.7 mL of LH-D reagent and 0.8 mL of LH-E reagent to each digestion tube and shake.
[0057] Make the liquid in the tube merge;
[0058] S5-3-3-4. Use a multi-parameter digestion instrument, select COD digestion, heat the machine to 165°C and then put the digestion tube in.
[0059] Digestion time: 10 min;
[0060] S5-3-3-5. After digestion is completed, wait for the test tube to cool down, take it out, and place it in a cooling tank to cool to room temperature;
[0061] S5-3-3-6. Add 2.5 mL of pure water to each of the cooled digestion tubes, shake the solution in each test tube thoroughly until there is no stratification and no flocs, shake evenly and place it in the cooling tank again to cool;
[0062] S5-3-3-7. After the multi-parameter water quality analyzer is preheated, select the corresponding measurement item, rinse the 30mm cuvette with pure water, pour the blank water sample into the cuvette, put it into the analyzer, and press the blank key to reset to zero after the reading stabilizes;
[0063] S5-3-3-8. Before each measurement, the cuvette must be rinsed with pure water, and each water sample to be tested must be measured in turn. The result displayed on the instrument is the COD concentration value.
[0064] The step S5 calculates the photocatalytic degradation efficiency of the photocatalytic porous concrete, and the calculation formula is as follows:
[0065]
[0066] Where: η is the photocatalytic degradation efficiency of TN, TP or COD; C0 is the initial concentration of TN, TP or COD; C t is the concentration of TN, TP or COD at time t.
[0067] The advantages of the present invention compared with the prior art are:
[0068] The method of the present application can obtain the optimal porosity of the photocatalytic concrete, the optimal concentration of the photocatalytic dispersion and the optimal spraying amount, so that the sewage treatment effect of the photocatalytic concrete is optimal. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1The present invention is a flow chart of a test method for photocatalytic porous concrete.
[0070] Figure 2 It is a line graph of the degradation of COD under different TiO2 concentrations according to a test method of photocatalytic porous concrete of the present invention.
[0071] Figure 3 It is a line graph of the degradation of TP under different TiO2 concentrations according to a test method for photocatalytic porous concrete of the present invention.
[0072] Figure 4 It is a line graph of the degradation of TN under different TiO2 concentrations according to a test method of photocatalytic porous concrete of the present invention.
[0073] Figure 5 It is a bar graph of the maximum degradation rate of various indicators with different concentrations of TiO2 in a test method for photocatalytic porous concrete of the present invention.
[0074] Figure 6 It is a line graph of the degradation of COD under different TiO2 spraying amounts according to a test method of photocatalytic porous concrete of the present invention.
[0075] Figure 7 It is a line graph showing the degradation of TP under different TiO2 spraying amounts according to a test method of photocatalytic porous concrete of the present invention.
[0076] Figure 8 It is a line graph showing the degradation of TN under different TiO2 spraying amounts according to a test method of photocatalytic porous concrete of the present invention.
[0077] Fig. 9 It is a bar graph of the maximum degradation rate of various indicators with different TiO2 spraying amounts in a test method for photocatalytic porous concrete of the present invention.
[0078] Fig.10 It is a line graph of the effect of target porosity on COD degradation efficiency in a test method for photocatalytic porous concrete of the present invention.
[0079] Fig.11 It is a line graph of the effect of target porosity on TN degradation efficiency in a test method for photocatalytic porous concrete of the present invention.
[0080] Fig.12 It is a line graph of the effect of target porosity on TP degradation efficiency in a test method for photocatalytic porous concrete of the present invention. DETAILED DESCRIPTION
[0081] The present invention provides a photocatalytic porous concrete, and the porous concrete surface is sprayed with nano-TiO2 dispersion. The porosity of the porous concrete is 6%-10%, and the materials of the porous concrete include coarse aggregate, fine aggregate, cementitious material and water. The coarse aggregate content is 12-15 times the water content, the fine aggregate content is 13.-1.6 times the water content, and the ratio of water to cementitious material is 0.3. The cementitious material includes cement, silica fume, water reducer and air entraining agent. The silica fume dosage is 8% of the cementitious material dosage. The water reducer is a polycarboxylic acid high-efficiency water reducer, and the water reducer parameter is 1% of the cementitious material dosage. The air entraining dosage is 0.1% of the cementitious material dosage. The spraying amount of the nano-TiO2 dispersion is 200-500g / m 2 , the concentration of nano-TiO2 dispersion is 8%-12%.
[0082] The present invention provides a test method for photocatalytic porous concrete, comprising the following steps:
[0083] S1. Pouring porous concrete with the same porosity to prepare photocatalytic porous concrete. The materials used include coarse aggregate, fine aggregate, cement, silica fume, water reducer, and air entraining agent. The coarse aggregate is limestone crushed stone from the quarry. The particle size distribution range and aggregate performance indicators meet the requirements of relevant standards. The specific basic parameters are shown in Table 1 below.
[0084] Nominal particle size (mm) <![CDATA[Bulk density (kg / m 3 )]]> <![CDATA[Apparent density (kg / m 3 )]]> Void ratio (%) Mud content (%) 5~10 1488 2680 44 0.7
[0085] Table 1 Basic parameters of coarse aggregate
[0086] The fine aggregate is river sand. The screening results and main physical properties are shown in Tables 2 and 3.
[0087] Square hole sieve hole side length (mm) Residual mass (g) Screen residue (%) Cumulative residue (%) 4.75 0 0 0 2.36 0 0 0 1.18 0 0 0 0.6 458 91.6 91.6 0.3 1.2 0.2 91.8 0.15 37 7.4 99.2
[0088] Table 2 Fine aggregate screening results
[0089]
[0090] Table 3 Main physical properties of fine aggregate Cement is ordinary Portland cement, and its main technical indicators are shown in Table 4.
[0091]
[0092] Table 4 Main technical indicators of cement
[0093] Silica fume is used to replace part of the cement, and the dosage is 8.0% of the amount of cementitious materials. The water reducer is a polycarboxylic acid high-efficiency water reducer in the form of white powder, easily soluble in water, with a water reduction rate of 25%, and the dosage is 1.0% of the amount of cementitious materials. The dosage of the air entraining agent is 0.1% of the amount of cementitious materials. Nano-TiO2 uses P25 nano-TiO2 powder produced by Degussa Company of Germany. It is a mixed crystal photocatalyst. The weight ratio of the two crystal forms of anatase and rutile is about 80%:20%. The specific technical indicators are shown in Table 5.
[0094]
[0095] Table 5 Technical indicators of nano-TiO2
[0096] The water used in the experiments was laboratory water.
[0097] The water-binder ratio was selected as 0.3 in this test, and the target porosity was set at 6%, 8%, and 10% respectively to improve the strength of porous concrete and facilitate the application of the research results in engineering practice. The mix design of ordinary porous concrete is as follows:
[0098] Table 6.
[0099]
[0100] Table 6 Ordinary porous concrete mix ratio
[0101] First, add the aggregate and 50% of the water into the mixer and stir for 30 seconds to ensure that the aggregate is evenly moistened; then add the cementitious material into the mixer and stir for 60 seconds to fully coat the surface of the aggregate; finally, add the remaining water and admixture, stir for 90 seconds and then discharge the material.
[0102] S1-1. Load the mixed concrete into the mold in three times, so that the thickness of each layer of concrete is the same. Use a tamping rod to vertically tamp 20 times from the edge to the center in a spiral direction for each layer. When tamping the bottom layer of concrete, make the tamping rod touch the bottom of the mold. When tamping each other layer, make the tamping rod insert about 20cm into the next layer of concrete, and pay attention to tamping the edges and corners tightly until the concrete fills the entire mold;
[0103] S1-2. Use a vibrating table to vibrate the concrete material after tamping for 3 seconds to make the concrete dense;
[0104] S1-3. After the vibration is completed, the excess concrete material is removed and smoothed to complete the pouring of the porous concrete in the mold;
[0105] S1-4. After the porous concrete is cast, it is covered with plastic film to prevent water loss from affecting cement hydration, thereby adversely affecting the strength of the porous concrete, and placed in a standard curing room with a temperature of (20±2)°C and a relative humidity of about 95% for curing;
[0106] S1-5. De-mould after standing in a standard curing room for 48 hours.
[0107] S2. Prepare nano-TiO2 dispersions of different concentrations, and spray the nano-TiO2 dispersions of each concentration evenly on each porous concrete to obtain a photocatalytic porous concrete, comprising the following steps:
[0108] S2-1. Stir the nano-TiO2 powder with water until dissolved;
[0109] S2-2 using a high shear emulsifier to disperse the solution for 10min, and then dispersed using an ultrasonic cleaner for 30min to obtain a nano-TiO2 dispersion;
[0110] S2-3. Spray the nano-TiO2 dispersion on the porous concrete, let it air dry for 24 hours, and then put it in the curing room for standard curing until 28 days.
[0111] S3. Install a UV light source in a water container, and prepare a certain concentration of wastewater to be degraded in the water container. Prepare the wastewater to be degraded by diluting the standard solutions of total nitrogen, total phosphorus, and COD to 2.0 mg / L, 0.4 mg / L, and 40 mg / L to simulate the water quality in the drainage ditch for experimental research; the reaction device used in this photocatalytic test is a simple laboratory-made test system. Use organic glass plates to make an uncovered box with a size of 40cm×40cm×15cm. Use the organic glass box as a water container to place photocatalytic porous concrete and prepared wastewater to be degraded; use a 45cm×45cm×25cm carton to cut and perforate a fixed tubular UV light source, and use 4 8W UV lamps with a UV wavelength of 365nm as the experimental light source, with a distance of 5cm between adjacent lamp tubes. Considering that the drainage ditch of farmland is drained in May, June, and July each year, according to the climatic conditions in the north, the characteristic UV irradiance is selected as (15±0.5)W / m 2The UV radiation intensity at different positions in the test device was measured using a UV irradiator. The UV radiation intensity reached a predetermined value by adjusting the height of the UV lamp. The UV lamp was finally determined to be 8 cm vertically above the water surface. A certain concentration of wastewater to be degraded was prepared in a plexiglass box, and the photocatalytic porous concrete was placed in the box and placed in the middle. After the carton was covered, the entire test system was completely covered with a blackout cloth to ensure the airtightness of the reaction device. All UV lamps were then turned on to start the photocatalytic degradation test. Water samples were taken every 20 minutes. The total duration of the photocatalytic reaction was determined to be 120 minutes through preliminary tests.
[0112] S4. placing each porous concrete in the wastewater to be degraded;
[0113] S5. After the photocatalytic reaction is completed, the nitrogen, phosphorus and chemical oxygen demand in the degraded wastewater are measured, and the photocatalytic degradation efficiency of the photocatalytic porous concrete sprayed with different concentrations of nano-TiO2 dispersion is calculated according to the measurement results, comprising the following steps:
[0114] S5-1. Use a pipette to collect water from the upper surface of the photocatalytic porous concrete in the water container. Take water samples three times at the diagonal and center points in each time period;
[0115] S5-2. Put the three water samples into polyethylene bottles respectively and record the numbers;
[0116] S5-3. After the photocatalytic reaction is completed, the pollutant characterization indicators are measured in time, and each water sample is measured 3 times, and the average value of the 3 measurements is taken as the final test result;
[0117] The total nitrogen (TN) content in the degradation wastewater is determined by the following steps:
[0118] S5-3-1-1. Prepare alkaline potassium persulfate solution and hydrochloric acid dilution used for testing nitrogen content;
[0119] S5-3-1-2. Use a pipette to take 5 mL of the water sample to be tested and inject it into a closed digestion tube. Add 5 mL of pure water to the blank group;
[0120] S5-3-1-3. Add 5 mL of alkaline potassium persulfate solution to each test tube, tighten the digestion tube cap, and shake the liquid in the digestion tube thoroughly;
[0121] S5-3-1-4. Turn on the multi-parameter digestion instrument, select TN digestion, heat the machine to 122°C, then put the digestion tube into the digestion tube and digest for 40 minutes;
[0122] S5-3-1-5. After digestion is completed, wait for the test tube to cool down slightly, take it out and place it on the test tube rack, and then put it into the cooling tank to cool;
[0123] S5-3-1-6. After cooling the test tubes to room temperature, add 1 mL of hydrochloric acid diluent, cover the test tubes tightly and shake well;
[0124] S5-3-1-7. Preheat the total nitrogen analyzer and select the sample for measurement; rinse the 10mm cuvette with pure water, pour the blank water sample into the cuvette first, put it into the measuring instrument, and press the blank key to reset to zero after the reading stabilizes;
[0125] S5-3-1-8. Test each water sample in turn, and rinse the cuvette with pure water before testing each water sample. The reading displayed when the cuvette is placed in the measuring instrument is the test result;
[0126] The total phosphorus TP content in the degradation wastewater is determined by the following steps:
[0127] S5-3-2-1. Prepare potassium persulfate, ammonium molybdate and ascorbic acid solution required for testing TP content;
[0128] S5-3-2-2. Use a pipette to take 8 mL of the water sample to be tested and inject it into a closed digestion tube. Add 8 mL of pure water to the blank group.
[0129] S5-3-2-3. After taking the water sample, add 1 mL of potassium persulfate solution to each digestion tube, cover the lid tightly, and shake the solution in the tube thoroughly;
[0130] S5-3-2-4. Select TP digestion on the multi-parameter digestion instrument startup page. After the machine heats up to 120°C, put the digestion tube in and start digestion.
[0131] S5-3-2-5. After digestion for 30 minutes, take out the test tube after it cools down, place it on a test tube rack and put it in a cooling tank to cool to room temperature;
[0132] S5-3-2-6. Take out the test tubes that have been digested and cooled to room temperature, add 1 mL of ascorbic acid solution and 1 mL of ammonium molybdate solution to each test tube, cover the test tubes tightly, shake well, and let stand for color development;
[0133] S5-3-2-7. Preheat the multi-parameter water quality analyzer, select the corresponding test item, first use pure water to rinse the 30mm cuvette, then pour the blank water sample into the cuvette, put it into the measuring instrument, and press the blank key to reset to zero after the reading stabilizes;
[0134] S5-3-2-8. After the instrument is set to zero, each sample to be tested is placed in turn, and the number displayed on the instrument is the test result;
[0135] The determination of the chemical oxygen demand (COD) content in the degradation wastewater includes the following steps:
[0136] S5-3-3-1. Use LH-D and LH-E powders to prepare LH-D reagent and LH-E reagent required for determining COD content;
[0137] S5-3-3-2. Take 2.5 mL of the water sample to be tested and inject it into an open digestion tube. Add 8 mL of pure water to the blank group.
[0138] S5-3-3-3. Add 0.7 mL of LH-D reagent and 0.8 mL of LH-E reagent to each digestion tube and shake.
[0139] Make the liquid in the tube merge;
[0140] S5-3-3-4. Use a multi-parameter digestion instrument, select COD digestion, heat the machine to 165°C and then put the digestion tube in.
[0141] Digestion time: 10 min;
[0142] S5-3-3-5. After digestion is completed, wait for the test tube to cool down, take it out, and place it in a cooling tank to cool to room temperature;
[0143] S5-3-3-6. Add 2.5 mL of pure water to each of the cooled digestion tubes, shake the solution in each test tube thoroughly until there is no stratification and no flocs, shake evenly and place it in the cooling tank again to cool;
[0144] S5-3-3-7. After the multi-parameter water quality analyzer is preheated, select the corresponding measurement item, rinse the 30mm cuvette with pure water, pour the blank water sample into the cuvette, put it into the analyzer, and press the blank key to reset to zero after the reading stabilizes;
[0145] S5-3-3-8. Before each measurement, the cuvette must be rinsed with pure water, and each water sample to be tested must be measured in turn. The result displayed on the instrument is the COD concentration value.
[0146] The photocatalytic degradation efficiency of photocatalytic porous concrete is calculated as follows:
[0147]
[0148] Where: η is the photocatalytic degradation efficiency of TN, TP or COD; C0 is the initial concentration of TN, TP or COD; C t is the concentration of TN, TP or COD at time t.
[0149] S6. The optimal concentration of nano-TiO2 dispersion was obtained based on the photocatalytic degradation efficiency; nano-TiO2 aqueous solutions with concentrations of 8%, 10%, and 12% were prepared and sprayed on the surface of porous concrete to prepare photocatalytic porous concrete, and sewage degradation tests were carried out using a photocatalytic test device. The optimal concentration of nano-TiO2 solution was obtained by analyzing the concentration changes of the three indicators of COD, TN, and TP and the photocatalytic degradation rate.
[0150] Through the photocatalytic degradation of pollutants in water, the effects of different concentrations of nano-TiO2 solutions on the photocatalytic degradation of COD, TN, and TP were obtained. The specific test results are as follows: Figure 2 As shown:
[0151] Figure 2 The effect of the concentration of nano-TiO2 solution on the COD degradation effect. The porous concrete without photocatalyst spraying uses its own porous characteristics to adsorb some pollutants, and the COD concentration drops to 38.37mg / L in 20 minutes. After 40 minutes, the adsorption equilibrium is basically reached, and the COD concentration drops to about 37.52mg / L; after 100 minutes of photocatalytic test, the concentration of COD in the water of the porous concrete sprayed with TiO2 solution basically reaches a dynamic equilibrium state; after 120 minutes of photocatalytic test, the porous concrete sprayed with a photocatalyst concentration of 10% has the highest COD degradation rate, and the COD concentration is 27.31mg / L at this time. Figure 3 It is the effect of TiO2 aqueous solution concentration on the degradation effect of pollutant TP. The adsorption capacity of porous concrete in the control group for TP reaches its limit at about 60 minutes, at which time the TP concentration is 0.342 mg / L; after 120 minutes of photocatalysis, the TP concentration of porous concrete sprayed with 8% concentration drops to 0.178 mg / L, and the TP concentration of porous concrete sprayed with 12% concentration drops to 0.201 mg / L; the photocatalytic concrete sprayed with 10% concentration has the greatest degree of TP degradation, and the TP concentration is 0.164 mg / L at 120 minutes. The effect of different concentrations of nano-TiO2 aqueous solution on the degradation effect of TN is shown in the figure. Figure 4 The porous concrete without photocatalyst reduces the TN concentration to 1.870 mg / L by adsorption capacity; under the photocatalytic action of 120 min, the porous concrete sprayed with 8%, 10%, and 12% nano-photocatalyst reduces the TN pollutant concentration to 1.501 mg / L and 1.451 mg / L respectively.
[0152] Depend on Figure 5It can be seen that the porous concrete without spraying photocatalytic materials has a small effect on the degradation of pollutants. By utilizing the adsorption of the porous concrete material itself, after 120 minutes of photocatalytic reaction, the degradation efficiency of TN and COD reaches about 6%, and the degradation rate of TP reaches about 14%. As the concentration of the photocatalyst increases, its degradation rate shows an increasing trend. When the concentration rises to 10%, the degradation efficiency of the photocatalytic porous concrete for each pollutant index reaches the maximum, among which the degradation effect on TP is the most obvious, with a degradation rate of 59%, and the degradation rates of TN and COD are 27.45% and 31.73% respectively.
[0153] In summary, the degradation rate of porous concrete sprayed with nano-titanium dioxide aqueous solution at a concentration of 10% is higher than that of photocatalytic porous concrete sprayed with concentrations of 8% and 12%. The reason may be that the number of nano-titanium dioxide particles in the 8% solution is small, the contact area with ultraviolet light is small, and the photocatalytic effect is slightly poor; the nano-titanium dioxide content in the 12% solution is too high, it is easy to agglomerate, and has a certain shielding effect, so the photocatalytic effect is also poor. Therefore, the above test results show that the optimal preparation concentration of nano-TiO2 aqueous solution is 10%.
[0154] S7. Prepare the nano-TiO2 dispersion with the best concentration, and spray it on each porous concrete with different spraying amounts. According to the test in the previous section, 10% photocatalyst is the best concentration. Therefore, this test uses a 10% nano-TiO2 aqueous solution to spray porous concrete, and the spraying amount is set to 200g / m 2 , 300g / m 2 , 500g / m 2 According to the concentration changes of each degradation index, the relationship between the photocatalytic degradation efficiency and the spraying amount was analyzed, and the optimal spraying amount of the nano-TiO2 solution was obtained.
[0155] S8. Repeat step S5 to obtain the optimal spraying amount of nano-TiO2 dispersion; the effect of the spraying amount of nano-TiO2 solution on the photocatalytic degradation of COD Figure 6 As shown. It can be seen from the figure that the greater the amount of photocatalytic solution sprayed, the lower the COD concentration in the sewage. This is because the more nano-TiO2 is used, the more electrons and holes are generated by photocatalysis, and the greater the degradation rate of organic matter. During the 120-minute photocatalytic test time, the photocatalytic porous concrete with a spraying amount of 500g / m2 showed the best degradation ability, which could reduce the COD concentration to 26.2mg / L; the porous concrete sprayed with 300g / m2 of photocatalytic material degraded the COD concentration to 27.3mg / L, also showing a good photocatalytic effect; the lowest degradation rate was the photocatalytic loading of 200g / m 2The porous concrete can degrade COD concentration to 32.2 mg / L. Figure 7 The figure shows the effect of different nano-TiO2 solution spraying amounts on the photocatalytic degradation of TP. Under the excitation of ultraviolet light, nano-TiO2 will react with organic phosphorus in sewage and degrade it into inorganic ions such as inorganic phosphorus and carbon dioxide, thereby achieving the effect of reducing total phosphorus pollutants in water. As can be seen from the figure, the photocatalytic solution spraying amount is 300g / m 2 and 500g / m 2 The degradation of TP by porous concrete was basically the same after 60 minutes of photocatalytic test. After the photocatalytic test, the concentration of TP in the sewage dropped to about 0.16 mg / L. In contrast, the porous concrete sprayed with 200 g / m 2 The photocatalytic ability of porous concrete is slightly poor, and the degradation TP concentration is 0.20 mg / L.
[0156] Figure 8 This is the effect of the amount of nano-TiO2 solution sprayed on the photocatalytic degradation of TN in water. In the photocatalytic reaction, nano-TiO2 is excited by ultraviolet light to cause ammonia nitrogen, nitrite nitrogen, nitrate nitrogen and hydroxide ions, hydrogen ions, electrons, etc. to react in series. Under the combined effect of this series of reactions, the TN concentration will eventually decrease. Photocatalytic tests were carried out on porous concrete with different amounts of TiO2 solution sprayed. As time went on, the TN concentration showed a trend of gradually decreasing. After 80 minutes of the test, the degradation of TN by various types of photocatalytic concrete began to reach a dynamic equilibrium state. After the photocatalytic test, the nano-photocatalyst loaded with 200g / m 2 , 300g / m 2 , 500g / m 2 The porous concrete reduced the TN pollutant concentration to 1.587 mg / L, 1.451 mg / L and 1.390 mg / L respectively.
[0157] Fig. 9 After 120 minutes of photocatalysis, porous concrete with different spraying amounts of nano-TiO2 solution shows the degradation of various characterization indicators. As can be seen from the figure, the degradation efficiency of photocatalytic porous concrete for various pollutants increases with the increase of the spraying amount of nano-TiO2 solution. The spraying amount is 200g / m 2 The degradation rate of various pollutants by the photocatalytic porous concrete is lower than that of the other two porous concretes; when the spraying amount is 500g / m 2 When the photocatalytic degradation efficiency is the best, the degradation rates of TN, COD and TP are 30.5%, 34.5% and 60.3% respectively; when the TiO2 solution is sprayed at 300g / m 2The degradation rates of TN, COD and TP by porous concrete are 27.5%, 31.7% and 59.0% respectively.
[0158] From the above analysis, it can be seen that the spraying amount of nano titanium dioxide is 300g / m 2 and 500g / m 2 The degradation efficiency of various indicators of photocatalytic porous concrete is significantly higher than that of the spraying amount of 200g / m 2 The porous concrete may be caused by 200g / m 2 The photocatalytic coating formed by the spraying amount is thinner, and the nano-titanium dioxide particles participating in the photocatalytic reaction are less, which leads to the degradation efficiency deviation of this photocatalytic concrete. The spraying amount is 300g / m 2 and 500g / m 2 The degradation efficiency of the photocatalytic porous concrete for various pollutants is not much different. Considering the economic efficiency of the practical application of photocatalytic materials, it is concluded that the optimal spraying amount of nano-TiO2 aqueous solution is 300g / m 2 .
[0159] S9. Cast porous concrete with different porosities, prepare nano-TiO2 dispersion with the best concentration, and spray the dispersion on each porous concrete with the best spraying amount; re-prepare a batch of porous concrete with porosities of 6%, 8%, and 10%, and a batch of porous concrete with porosities of 6%, 8%, and 10%, a TiO2 concentration of 10%, and a TiO2 spraying amount of 200g / m 2 , 300g / m 2 and 500g / m 2 The photocatalytic porous concrete was prepared, and the porosity was tested according to the relevant provisions of the "Technical Specification for Application of Recycled Aggregate Permeable Concrete" (CJJ / T 253-2016), the permeability coefficient was tested according to the "Technical Specification for Permeable Cement Concrete Pavement" (CJJ / T 135-2009), and the compressive strength was tested according to the relevant regulations in the "Standard for Test Methods for Physical and Mechanical Properties of Concrete" (GB / T50081-2019). The results are shown in Table 7:
[0160]
[0161] Through comprehensive analysis of the above data, it can be concluded that the spraying of nano-TiO2 materials can reduce porosity, permeability and improve compressive strength to a certain extent, but this effect is not obvious and can be ignored.
[0162] The porosity of concrete has a certain influence on the contact area between the concrete surface and the outside world. The degradation test of ordinary concrete sprayed with photocatalytic materials with a relatively smooth surface used in most channel linings was carried out as a control group, and the photocatalytic degradation of TN, TP, and COD of photocatalytic porous concrete with different target porosities was studied to analyze the influence of concrete porosity on the degradation rate.
[0163] S10. Repeat step S5 to obtain the optimal porosity of the porous concrete. The degradation of COD by photocatalytic porous concrete with different porosities is shown in Fig.10 As shown in the figure, with the increase of the target porosity of porous concrete, the degradation efficiency of COD by photocatalytic porous concrete gradually decreases. After 120 minutes of photocatalytic reaction, the photocatalytic porous concrete with target porosity of 6%, 8%, and 10% degraded COD by 31.73%, 34.65%, and 36.83%, respectively. The degradation rate of COD by photocatalytic ordinary concrete was only 14.23%.
[0164] Fig.11 As for the influence of porosity on the TN degradation effect, under the photocatalytic reaction time of 120 minutes, the photocatalytic porous concrete with a target porosity of 10% has the highest TN degradation rate, which can reach about 30%; the degradation rates of porous concrete with porosities of 6% and 8% are slightly lower, both at about 28%; the degradation efficiency of ordinary photocatalytic concrete for TN is about 13%.
[0165] Depend on Fig.12It can be seen that the degradation of TP by photocatalytic porous concrete with different target porosities tends to be consistent and gradually reaches dynamic equilibrium after 80 minutes of photocatalytic reaction, and the final degradation rate reaches about 60%; the degradation efficiency of ordinary photocatalytic concrete gradually increases with the increase of time, and the degradation rate of TP reaches 29.75% after the reaction. Comprehensive analysis of the above test results shows that when ordinary concrete loaded with nano-TiO2 solution is used for photocatalytic test, its degradation efficiency of sewage is lower than that of photocatalytic porous concrete. After 120 minutes of photocatalytic reaction time, the degradation efficiency of TN, TP and COD by ordinary photocatalytic concrete can only reach about 49%, 50% and 45% of the degradation rate of photocatalytic porous concrete with a target porosity of 6%. It can be concluded that using the characteristics of porous concrete with large porosity and rough surface to photocatalytically degrade pollutants in water can obtain more significant test results. This is due to the special surface structure of porous concrete, which allows the sprayed photocatalyst solution to adhere to the concrete surface and gaps as much as possible, thereby increasing the photocatalytic reaction area and making the photocatalytic performance of porous concrete better than that of ordinary concrete, which can show a better degradation effect in practical applications. Therefore, under the premise of meeting the mechanical properties of porous concrete, the porosity of porous concrete should be increased as much as possible to achieve the maximum degradation rate of water pollutants.
[0166] The present invention is described by way of embodiments, and those skilled in the art will appreciate that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application belong to the protection scope of the present invention.
Claims
1. A photocatalytic porous concrete, characterized in that: Spraying nano-TiO2 dispersion on the porous concrete surface.
2. The photocatalytic porous concrete according to claim 1, characterized in that: The porosity of the porous concrete is 6%-10%. The materials of the porous concrete include coarse aggregate, fine aggregate, cementitious material and water, and the ratio of coarse aggregate: fine aggregate: cementitious material: water is (12-15): (1.3-1.6): 3.3:
1.
3. The photocatalytic porous concrete according to claim 2, characterized in that: The cementitious material comprises cement, silica fume, water reducing agent and air entraining agent, wherein the silica fume content is 8% of the total cementitious material, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, the water reducing agent parameter is 1% of the total cementitious material, and the air entraining content is 0.1% of the total cementitious material.
4. The photocatalytic porous concrete according to claim 1, characterized in that: The spraying amount of the nano-TiO2 dispersion is 200-500g / m 2 , the concentration of nano-TiO2 dispersion is 8%-12%.
5. A test method for photocatalytic porous concrete, characterized in that: The following steps are involved: S1. pouring porous concrete with the same porosity; S2 configuration of different concentrations of nano-TiO2 dispersion, and each concentration of nano-TiO2 dispersion were sprayed evenly on each porous concrete to obtain a photocatalytic porous concrete; S3. Install a UV light source in the water container and configure a certain concentration of wastewater to be degraded in the water container; S4. placing each porous concrete in the wastewater to be degraded; S5. After the photocatalytic reaction is completed, the nitrogen, phosphorus and chemical oxygen demand in the degraded wastewater are measured, and the photocatalytic degradation efficiency of the photocatalytic porous concrete sprayed with different concentrations of nano-TiO2 dispersion is calculated based on the measurement results; S6. The optimal concentration of nano-TiO2 dispersion is obtained according to the photocatalytic degradation efficiency; S7 configure the optimal concentration of nano-TiO2 dispersion, and the dispersion was sprayed on each porous concrete in different spraying amounts; S8. Repeat step S5 to obtain the optimal spraying amount of nano-TiO2 dispersion; S9. Pouring porous concrete of different porosities, configuring the optimal concentration of nano-TiO2 dispersion, and spraying the dispersion on each porous concrete at the optimal spraying amount; S10. Repeat step S5 to obtain the optimal porosity of the porous concrete.
6. The test method of photocatalytic porous concrete according to claim 5, characterized in that: The step S1 of pouring porous concrete with the same porosity comprises the following steps: S1-1. The mixed concrete material is loaded into the mold so that each layer of concrete material has the same thickness. Each layer is loaded with a tamping rod from the edge to the center of the spiral tamping. When the bottom layer of concrete material is tamped, the tamping rod touches the bottom of the mold. When each layer is tamped, the tamping rod is inserted into the next layer of concrete material; S1-2. Use a vibrating table to vibrate the concrete material after tamping; S1-3. After the vibration is completed, the excess concrete material is removed and smoothed to complete the pouring of the porous concrete in the mold; S1-4. After the porous concrete is cast, it is covered with a plastic film and placed in a standard curing room at a temperature of (20±2)°C and a relative humidity of 95% for curing; S1-5. De-mould after standing in a standard curing room for 48 hours.
7. The test method of photocatalytic porous concrete according to claim 5, characterized in that: The step S2 of preparing a nano-TiO2 dispersion and spraying it on the porous concrete comprises the following steps: S2-1. Stir the nano-TiO2 powder with water until dissolved; S2-2 using a high shear emulsifier to disperse the solution, and then dispersed using an ultrasonic cleaner to obtain a nano-TiO2 dispersion; S2-3. Spray the nano-TiO2 dispersion on the porous concrete, let it air dry for 24 hours, and then put it in the curing room for standard curing until 28 days.
8. The test method of photocatalytic porous concrete according to claim 5, characterized in that: The ultraviolet irradiance of the ultraviolet light source in step S3 is (15±0.5) W / m 2 .
9. The test method of photocatalytic porous concrete according to claim 5, characterized in that: The step S5 of measuring nitrogen, phosphorus and chemical oxygen demand in the degradation wastewater comprises the following steps: S5-1. Use a pipette to collect water from the upper surface of the photocatalytic porous concrete in the water container. Take water samples three times at the diagonal and center points in each time period; S5-2. Put the three water samples into polyethylene bottles respectively; S5-3. Each water sample was tested three times, and the average of the three tests was taken as the final test result; The total nitrogen (TN) content in the degradation wastewater is determined by the following steps: S5-3-1-1. Prepare alkaline potassium persulfate solution and hydrochloric acid dilution used for testing nitrogen content; S5-3-1-2. Use a pipette to take 5 mL of the water sample to be tested and inject it into a closed digestion tube. Add 5 mL of pure water to the blank group; S5-3-1-3. Add 5 mL of alkaline potassium persulfate solution to each test tube, tighten the digestion tube cap, and shake the liquid in the digestion tube thoroughly; S5-3-1-4. Turn on the multi-parameter digestion instrument, select TN digestion, heat the machine to 122°C, then put the digestion tube into the digestion tube and digest for 40 minutes; S5-3-1-5. After digestion is completed, wait for the test tube to cool down slightly, take it out and place it on the test tube rack, and then put it into the cooling tank to cool; S5-3-1-6. After cooling the test tubes to room temperature, add 1 mL of hydrochloric acid diluent, cover the test tubes tightly and shake well; S5-3-1-7. Preheat the total nitrogen analyzer and select the sample for measurement; rinse the 10mm cuvette with pure water, pour the blank water sample into the cuvette first, put it into the measuring instrument, and press the blank key to reset to zero after the reading stabilizes; S5-3-1-8. Test each water sample in turn, and rinse the cuvette with pure water before testing each water sample. The reading displayed when the cuvette is placed in the measuring instrument is the test result; The total phosphorus TP content in the degradation wastewater is determined by the following steps: S5-3-2-1. Prepare potassium persulfate, ammonium molybdate and ascorbic acid solution required for testing TP content; S5-3-2-2. Use a pipette to take 8 mL of the water sample to be tested and inject it into a closed digestion tube. Add 8 mL of pure water to the blank group. S5-3-2-3. After taking the water sample, add 1 mL of potassium persulfate solution to each digestion tube, cover the lid tightly, and shake the solution in the tube thoroughly; S5-3-2-4. Select TP digestion on the multi-parameter digestion instrument startup page. After the machine heats up to 120°C, put the digestion tube in and start digestion. S5-3-2-5. After digestion for 30 minutes, take out the test tube after it cools down, place it on a test tube rack and put it in a cooling tank to cool to room temperature; S5-3-2-6. Take out the test tubes that have been digested and cooled to room temperature, add 1 mL of ascorbic acid solution and 1 mL of ammonium molybdate solution to each test tube, cover the test tubes tightly, shake well, and let stand for color development; S5-3-2-7. Preheat the multi-parameter water quality analyzer, select the corresponding test item, first use pure water to rinse the 30mm cuvette, then pour the blank water sample into the cuvette, put it into the measuring instrument, and press the blank key to reset to zero after the reading stabilizes; S5-3-2-8. After the instrument is set to zero, each sample to be tested is placed in turn, and the number displayed on the instrument is the test result; The determination of the chemical oxygen demand (COD) content in the degradation wastewater includes the following steps: S5-3-3-1. Use LH-D and LH-E powders to prepare LH-D reagent and LH-E reagent required for determining COD content; S5-3-3-2. Take 2.5 mL of the water sample to be tested and inject it into an open digestion tube. Add 8 mL of pure water to the blank group. S5-3-3-3. Add 0.7 mL of LH-D reagent and 0.8 mL of LH-E reagent to each digestion tube, and shake to mix the liquid in the tube; S5-3-3-4. Use a multi-parameter digestion instrument, select COD digestion, heat the machine to 165°C and then put in the digestion tube, digestion time 10 minutes; S5-3-3-5. After digestion is completed, wait for the test tube to cool down, take it out, and place it in a cooling tank to cool to room temperature; S5-3-3-6. Add 2.5 mL of pure water to each of the cooled digestion tubes, shake the solution in each test tube thoroughly until there is no stratification and no flocs, shake evenly and place it in the cooling tank again to cool; S5-3-3-7. After the multi-parameter water quality analyzer is preheated, select the corresponding measurement item, rinse the 30mm cuvette with pure water, pour the blank water sample into the cuvette, put it into the analyzer, and press the blank key to reset to zero after the reading stabilizes; S5-3-3-8. Before each measurement, the cuvette must be rinsed with pure water, and each water sample to be tested must be measured in turn. The result displayed on the instrument is the COD concentration value.
10. The test method of photocatalytic porous concrete according to claim 5, characterized in that: The step S5 calculates the photocatalytic degradation efficiency of the photocatalytic porous concrete, and the calculation formula is as follows: Where: η is the photocatalytic degradation efficiency of TN, TP or COD; C0 is the initial concentration of TN, TP or COD; C t is the concentration of TN, TP or COD at time t.
Citation Information
Patent Citations
Concrete material having function of purifying gas-solid pollutants and preparation method thereof
CN102850017A
Durable concrete photocatalysis slurry and concrete capable of removing NOx (oxynitride)
CN107176820A
Multi-pore cement concrete with photocatalytic purification effect
CN109987967A
TiO2 polymer spray coating, photocatalytic regenerated pervious concrete containing TiO2 polymer spray coating and preparation method of photocatalytic regenerated pervious concrete
CN118085620A
Composition of conductive photocatalytic concrete for improving durability and its preparation method