Method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas

By using methanol as an absorber and composite modified material as adsorption filler in coal-to-ethanol vent recovery, the problems of high energy consumption and low purity of dimethyl ether are solved, and the preparation and cost reduction of high purity dimethyl ether are achieved .

CN118955252AInactive Publication Date: 2024-11-15ANHUI CARBON XIN TECH CO LTD

Patent Information

Application Number
CN202411446608.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the energy consumption and production cost of coal-to-ethanol recovery in the preparation of dimethyl ether is high, and the purity of dimethyl ether needs to be improved.

Method used

Methanol is used as the absorption solvent, and the venting gas is absorbed through the spray tower, and the composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth and silicate solution are soaked in the plate-type distillation tower. The polyurethane foam balls are used as adsorption filler to optimize the distillation tower parameters and achieve separation of dimethyl ether and impurities.

Benefits of technology

It effectively reduces the energy consumption of dimethyl ether distillation and purification, improves the purity of dimethyl ether, and reduces production costs by recycling methanol, and prepares high-purity dimethyl ether products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955252A_ABST
    Figure CN118955252A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, belongs to the technical field of dimethyl ether recovery and purification, and is used for solving the technical problems that in the prior art, the production cost of dimethyl ether prepared by recovering the ethanol purge gas is high, and the purity of the recovered dimethyl ether needs to be further improved. The method comprises the following steps: filtering ethanol purge gas through a filter to remove mechanical impurities so as to obtain pretreated purge gas, conveying the pretreated purge gas from the bottom of a methanol spray tower to the spray tower, and after the pretreated purge gas is adsorbed by methanol, recycling the ethanol purge gas. The composite modified metal powder, the modified zirconium metal powder, the modified diatomite and the silicate solution are used as dip dyeing solutions to dip dye polyurethane foam microspheres to prepare an adsorption filler with a high specific surface area, and a high-purity dimethyl ether product is prepared by optimizing a rectification process and promoting separation of impurities and dimethyl ether, so that the production energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of dimethyl ether recovery and purification, and in particular to a method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas. Background Art

[0002] Coal-to-ethanol uses coal-based synthesis gas as raw material, and mainly goes through the steps of synthesis gas to methanol, methanol dehydration to dimethyl ether, dimethyl ether carbonylation to methyl acetate, and methyl acetate hydrogenation to ethanol. Compared with the methanol carbonylation route, the dimethyl ether route does not require the use of reactors with high corrosion resistance, which reduces operating costs. At the same time, methyl acetate and methanol can also be sold as intermediate products, making it convenient for enterprises to switch to other products when ethanol is not profitable. However, the conversion rate of methanol is low, and the crude dimethyl ether generated needs to be distilled and separated, and the methanol needs to be recovered.

[0003] Due to the low boiling point of dimethyl ether, the dimethyl ether tail gas discharged from the top of the separation tower reflux tank still contains a considerable proportion of dimethyl ether (about 43% of the total purge gas). This part of the purge gas is mainly fed into the gas pipeline network after passing through the tail gas heater for direct combustion, which is bound to cause waste of resources and increase CO2 emissions.

[0004] In the prior art, the components of the purge gas after condensation of the top material of the dimethyl ether separation tower mainly include dimethyl ether, carbon dioxide, hydrogen, methane, ethylene and propylene. The dimethyl ether in the purge gas is absorbed by water, which can effectively remove insoluble impurities such as methane, ethylene and propylene. However, due to the large specific heat capacity of water, a large amount of energy is required when distilling and purifying dimethyl ether, and the energy consumption of dimethyl ether purification is high. Although the use of alcohol as an absorbent can effectively absorb dimethyl ether, at the same time, since the impurities in the purge gas have similar physical properties to dimethyl ether, traditional adsorption fillers are difficult to fully separate the impurities from dimethyl ether during the distillation process, resulting in the purity of dimethyl ether to be further improved.

[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the Invention

[0006] The object of the present invention is to provide a method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, so as to solve the technical problems in the prior art of recovering dimethyl ether prepared from ethanol purge gas, such as high energy consumption and high production cost, and the need to further improve the purity of the recovered dimethyl ether.

[0007] The object of the present invention can be achieved by the following technical solution: A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0008] S1. Filter the ethanol off-gas through a filter to remove mechanical impurities to obtain pretreated off-gas;

[0009] S2, transporting the pretreated purge gas from the bottom of the methanol spray tower to the spray tower, and obtaining the purge waste gas and methanol extract after methanol adsorption;

[0010] S3, adding the composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth, and silicate solution into a reaction kettle and stirring evenly to obtain an immersion dye, adding polyurethane foam balls into the immersion dye, squeezing out bubbles in the polyurethane foam balls, draining, and then putting them into the immersion dye, repeating the immersion dyeing operation 8-10 times, and post-processing to obtain an adsorption filler;

[0011] S4. Fill a tray-type distillation tower with an adsorption filler, deliver the methanol extract to the distillation tower from a feed pipe, and set the reflux ratio inside the distillation tower to 2.6-2.8 and the pressure to 0.6-0.8 MPa;

[0012] S5. After being processed in the distillation tower, the finished dimethyl ether is extracted from the top of the distillation tower, and the methanol is extracted from the methanol pipe at the top of the distillation tower and transported to the heat exchanger for cooling and heat exchange to obtain regenerated methanol. The regenerated methanol is transported to the methanol spray tower through the pipeline network for recycling.

[0013] Furthermore, in step S2, the gas-liquid ratio of the pre-treated purge gas to methanol is 1 cm 3 : 3-5mL; in step S4, the number of plates of the distillation tower is 80, and the position of the feed pipe is above the 16th plate from bottom to top; in step S5, the position of the methanol tube is above the 75th plate from bottom to top.

[0014] Furthermore, in step S3, the amount ratio of the composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth, and silicate solution is 3g:2g:5g:40mL, the silicate solution is composed of sodium silicate, polydiallyldimethylammonium chloride, and purified water in an amount ratio of 1g:3g:10mL, and the amount ratio of the impregnated dye and polyurethane foam ball is 7g:2-3cm 3 The size of the polyurethane foam balls is 5-8 mm, and the post-processing includes: after repeated impregnation is completed, the polyurethane foam balls are removed from the impregnation liquid and placed in a freeze dryer for freeze drying to constant weight, and then the dry embryo obtained by freeze drying is placed in a muffle furnace, the muffle furnace is raised to 600° C. at a rate of 1° C. / min, and after keeping the temperature for 2 hours, it is further raised to 850-900° C. at a rate of 5° C. / min, kept warm for 3 hours, taken out, cooled and discharged to obtain an adsorption filler.

[0015] Furthermore, the preparation method of the composite modified metal powder is: add scandium nitrate, cobalt nitrate, 3,3',4,4'-biphenyltetracarboxylic acid, and N,N,-dimethylformamide to a nitrogen-protected high-pressure reactor and stir until the system is dissolved, add hydrogen peroxide and pyridine to the high-pressure reactor, and pass a heat exchange medium with a temperature of 220-240°C into the jacket of the high-pressure reactor. After the pressure of the high-pressure reactor is balanced, keep warm and stir for 40-50 hours, and post-treat to obtain the composite modified metal powder.

[0016] The synthetic reaction mechanism of composite modified metal powder is:

[0017] Scandium nitrate and cobalt nitrate are dissolved in N,N,-dimethylformamide to release Sc 3+ and Co 2+ The ionic ligand, 3,3',4,4'-biphenyltetracarboxylic acid, is dissolved in N,N,-dimethylformamide and partially deprotonated to form negatively charged carboxyl ligands. These carboxyl ligands react with metal ion ligands to form metal-organic complexes. The hydrogen ions produced by the decomposition of hydrogen peroxide help balance the charge in the reaction system. Pyridine, as an organic base, can further promote the deprotonation of 3,3',4,4'-biphenyltetracarboxylic acid. The nitrogen atoms contained in the pyridine molecular structure can coordinate with metal ions to form a more complex complex structure, thereby preparing a composite modified metal powder.

[0018] Furthermore, the amount ratio of scandium nitrate, cobalt nitrate, 3,3',4,4'-biphenyltetracarboxylic acid, N,N,-dimethylformamide, hydrogen peroxide and pyridine is 7g:3g:5g:100mL:5mL:15mL, the mass fraction of the hydrogen peroxide is 25-30%, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the reactor is opened, and the filter cake is washed with N,N-dimethylformamide and anhydrous ethanol three times in sequence and then dried, and the filter cake is transferred to a drying oven at a temperature of 50-60°C and dried to constant weight to obtain a composite modified metal powder.

[0019] Furthermore, the preparation method of the modified zirconium metal powder is: adding anhydrous zirconium chloride, 2-amino-1,4-dicarboxylic acid and deionized water into a reactor and stirring, raising the temperature of the reactor to 95-100°C, keeping the temperature under reflux for 26-28 hours, and post-treating to obtain the modified zirconium metal powder.

[0020] The synthetic reaction mechanism of modified zirconium metal powder is:

[0021] During the reaction, the oxygen atom on the carboxyl group of 2-amino-1,4-dicarboxylic acid and the nitrogen atom on the amino group provide lone pairs of electrons to form coordination bonds with the empty orbitals of the zirconium ion, causing the zirconium ion to transform from a hydrated ion state to a complex coordination compound, thereby forming a modified zirconium metal powder of a zirconium-organic complex.

[0022] Furthermore, the usage ratio of anhydrous zirconium chloride, 2-amino-1,4-dicarboxylic acid and deionized water is 1g:1.5g:10mL. The post-treatment includes, after the reaction is completed, lowering the temperature of the reactor to 10-15°C, filtering, soaking the filter cake in anhydrous ethanol, ultrasonically dispersing for 60 minutes, filtering, placing the filter cake in a drying oven at a temperature of 50-60°C, and drying to constant weight to obtain modified zirconium metal powder.

[0023] Furthermore, the modified diatomaceous earth is obtained by processing the following steps:

[0024] A1. Add diatomaceous earth, tetrapropylammonium hydroxide and purified water into a reactor, stir at room temperature for 3-4 hours, and post-treat to obtain pretreated diatomaceous earth;

[0025] A2. Add the pretreated diatomaceous earth and the modified liquid into a reactor and stir. Pass a heat exchange medium at a temperature of 110°C into the jacket of the reactor and stir until the system temperature is balanced. Keep stirring for 72-78 hours and post-treat to obtain modified diatomaceous earth.

[0026] The synthetic reaction mechanism of modified diatomite is:

[0027] The tetrapropylammonium cation portion separated from tetrapropylammonium hydroxide in water undergoes physical adsorption on the surface of diatomite to prepare pretreated diatomite. After the pretreated diatomite is mixed with the modification liquid, it is stirred at high temperature to promote the hydrolysis and polycondensation reaction of ethyl orthosilicate, and a layer of silicon-oxygen network is covered on the surface of the diatomite. During the reaction, the tetrapropylammonium cation combines with the negative charge sites in the silicon-oxygen network through hydrogen bonding, further stabilizing the structure of the modified diatomite. The high-temperature treatment removes residual tetrapropylammonium hydroxide and other organic impurities, while promoting the rearrangement and solidification of the silicon-oxygen network, adjusting and optimizing the internal pore structure of the diatomite, and improving the adsorption performance and mechanical strength of the modified diatomite.

[0028] Furthermore, in step A1, the amount ratio of the diatomaceous earth, tetrapropylammonium hydroxide and purified water is 5g:1g:50mL, and the post-treatment includes: after the reaction is completed, filtering, rinsing the filter cake with purified water and then drying, transferring the filter cake to a drying oven at a temperature of 70-80°C, and drying to constant weight to obtain pretreated diatomaceous earth; in step A2, the amount ratio of the pretreated diatomaceous earth and the modifying liquid is 1g:10mL, and the modifying liquid is composed of ethyl orthosilicate, tetrapropylammonium hydroxide and purified water in an amount ratio of 3g:1g:5mL. The post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtering, washing the filter cake with purified water 3 times and then drying, placing the filter cake in a drying oven at a temperature of 70-80°C and drying it to constant weight, then transferring it to a muffle furnace, raising the temperature of the muffle furnace to 550-600°C, keeping it warm and calcining it for 6-8h, cooling and discharging it to obtain modified diatomaceous earth.

[0029] The present invention has the following beneficial effects:

[0030] 1. The method of the present invention for recovering and purifying dimethyl ether from the purge gas of coal-to-ethanol uses methanol as an absorption solvent, absorbs the purge gas through a spray tower, and performs distillation treatment on the methanol absorbed by the dimethyl ether in a distillation tower to separate the dimethyl ether from the methanol, impurities, etc., to prepare high-purity dimethyl ether. By replacing traditional water with methanol as the absorption solvent, the energy consumption of dimethyl ether distillation and purification can be effectively reduced, and the separated methanol can be recycled through a pipeline, effectively reducing the production cost. A multi-metal composite porous adsorption filler is filled in the distillation tower, and the adsorption filler is used as the packing bed of the distillation tower. The distillation parameters of the distillation tower are optimized, and the separation of methanol and impurities from dimethyl ether is promoted to prepare a high-purity dimethyl ether product.

[0031] 2. The method of the present invention for recovering and purifying dimethyl ether from coal-to-ethanol purge gas comprises impregnating polyurethane foam microspheres with a composite modified metal powder of scandium and cobalt coordinated with 3,3',4,4'-biphenyltetracarboxylic acid, a modified zirconium metal powder coordinated with 2-amino-1,4-dicarboxylic acid, modified diatomaceous earth, and a silicate solution as an impregnation solution, and then calcining the mixture at high temperature to prepare a porous adsorption filler with a high specific surface area; scandium and cobalt are both rare earth elements, and scandium has a smaller ion radius. , has high electrophilicity, which makes it have a strong affinity for weakly polar molecules such as methane, ethylene, and propylene. The cobalt ion has multiple unpaired electrons. Scandium and cobalt are coordinated with 3,3',4,4'-biphenyltetracarboxylic acid, which optimizes the pore size distribution, pore shape and surface chemical properties of the composite material, promotes the diffusion and adsorption of gas molecules such as methanol, methane, ethylene, and propylene in the pores, and at the same time limits the entry of larger molecules such as dimethyl ether, thereby showing selective permeability to dimethyl ether.

[0032] 3. The method of the present invention for recovering and purifying dimethyl ether from the off-gas of coal-to-ethanol production comprises a method for generating a zirconium-based complex or polymer by a coordination reaction between anhydrous zirconium chloride and the carboxyl and amino groups contained in 2-amino-1,4-dicarboxylic acid, thereby forming a zirconium-based material with a three-dimensional network structure, which provides abundant surface sites and pores for the adsorption of gas molecules. During the preparation process, the pore size and distribution of the zirconium-based material are adjusted by controlling the reaction conditions. A smaller pore size is conducive to the adsorption of small molecules such as methane, thereby maintaining a lower adsorption capacity for dimethyl ether and further promoting the adsorption of small molecule impurities. The separation of dimethyl ether from large molecules improves the recovery purity of dimethyl ether; the porous structure of diatomaceous earth itself is an important basis for it to be used as an adsorption material. Through modification treatment with the modifying liquid, the pore size of the diatomaceous earth is further expanded or refined, the porosity of the diatomaceous earth is improved, and the hydroxyl content on the surface of the diatomaceous earth modified by the modifying liquid is enhanced. These hydroxyl groups can form hydrogen bonds or other interactions with gas molecules, thereby enhancing the adsorption capacity. Through high-temperature calcination treatment, the interaction between silicon-oxygen bonds is enhanced, making the pore structure more solid and improving the durability of the adsorption filler. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0034] Figure 1 The present invention is a process flow chart for recovering and purifying dimethyl ether from ethanol purge gas;

[0035] Figure 2 is the XRD pattern of the composite modified metal powder in the present invention;

[0036] Figure 3 is the XRD pattern of the modified zirconium metal powder in the present invention;

[0037] Figure 4 is the XRD pattern of the modified diatomite in the present invention. DETAILED DESCRIPTION

[0038] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0039] Example 1

[0040] This embodiment provides a method for preparing an adsorption filler for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0041] S1. Preparation of composite modified metal powder

[0042] Weigh: 35 g of scandium nitrate hexahydrate, 15 g of cobalt nitrate hexahydrate, 25 g of 3,3',4,4'-biphenyltetracarboxylic acid, and 500 mL of N,N,-dimethylformamide, add them to a nitrogen-protected high-pressure reactor and stir until the system is dissolved. Add 25 mL of 25 wt% hydrogen peroxide and 75 mL of pyridine to the high-pressure reactor, and introduce a heat exchange medium with a temperature of 220°C into the jacket of the high-pressure reactor. After the pressure of the high-pressure reactor is balanced, keep warm and stir for 40 hours. The temperature of the reactor is lowered to room temperature, the reactor is opened, and the filter cake is filtered. The filter cake is washed three times with N,N-dimethylformamide and anhydrous ethanol in sequence and then dried. The filter cake is transferred to a drying oven at a temperature of 50°C and dried to constant weight to obtain a composite modified metal powder.

[0043] S2. Preparation of modified zirconium metal powder

[0044] Weigh: 40 g of anhydrous zirconium chloride, 60 g of 2-amino-1,4-dicarboxylic acid and 400 mL of deionized water are added to a reactor and stirred. The temperature of the reactor is raised to 95°C and refluxed for 26 hours. The temperature of the reactor is lowered to 10°C and filtered. The filter cake is immersed in anhydrous ethanol and ultrasonically dispersed for 60 minutes. The filter cake is filtered and placed in a drying oven at 50°C and dried to constant weight to obtain modified zirconium metal powder.

[0045] S3. Preparation of modified diatomite

[0046] Weigh: 50 g of diatomaceous earth, 10 g of tetrapropylammonium hydroxide and 500 mL of purified water were added to a reactor, stirred at room temperature for 3 h, filtered, the filter cake was rinsed with purified water and then dried, and the filter cake was transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain pretreated diatomaceous earth;

[0047] Ethyl orthosilicate, tetrapropylammonium hydroxide, and purified water were mixed uniformly in a ratio of 3 g:1 g:5 mL to obtain a modified solution;

[0048] The pretreated diatomaceous earth and the modified liquid were added to the reactor at a ratio of 1 g:10 mL and stirred. A heat exchange medium at a temperature of 110°C was introduced into the jacket of the reactor and stirred until the system temperature was balanced. The mixture was kept warm and stirred for 72 hours. The temperature of the reactor was lowered to room temperature and filtered. The filter cake was washed three times with purified water and then dried. The filter cake was placed in a drying oven at a temperature of 70°C and dried to constant weight. It was then transferred to a muffle furnace, the temperature of the muffle furnace was raised to 550°C, the mixture was kept warm and calcined for 6 hours, and the temperature was lowered and discharged to obtain modified diatomaceous earth.

[0049] S4. Preparation of immersion dye

[0050] Sodium silicate, polydiallyldimethylammonium chloride, and purified water were mixed uniformly in a ratio of 1 g:3 g:10 mL to obtain a silicate solution;

[0051] The composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth and silicate solution were added into a reaction kettle in a dosage ratio of 3g:2g:5g:40mL and stirred evenly to obtain an impregnation dye.

[0052] S5. Prepare adsorption filler.

[0053] Mix the dye and polyurethane foam balls with a size of 5-8mm in a ratio of 7g:2cm 3 , add it to a beaker and mix evenly, squeeze out the bubbles in the polyurethane foam ball, drain it, and then put it into the dye, repeat the dyeing operation 8 times, take the polyurethane foam ball out of the dyeing liquid and place it in a freeze dryer at a temperature of -30°C, freeze-dry it to constant weight, and then place the dry embryo obtained by freeze drying in a muffle furnace, and the muffle furnace is raised to 600°C at a rate of 1°C / min, and after keeping warm for 2 hours, it is continuously raised to 850°C at a rate of 5°C / min, and taken out after keeping warm for 3 hours, cooled and discharged to obtain an adsorption filler.

[0054] Example 2

[0055] This embodiment provides a method for preparing an adsorption filler for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0056] S1. Preparation of composite modified metal powder

[0057] Weigh: 35 g of scandium nitrate hexahydrate, 15 g of cobalt nitrate hexahydrate, 25 g of 3,3',4,4'-biphenyltetracarboxylic acid, and 500 mL of N,N,-dimethylformamide, add them to a nitrogen-protected high-pressure reactor and stir until the system is dissolved. Add 25 mL of 27 wt% hydrogen peroxide and 75 mL of pyridine to the high-pressure reactor, and introduce a heat exchange medium with a temperature of 230 ° C into the jacket of the high-pressure reactor. After the pressure of the high-pressure reactor is balanced, keep warm and stir for 45 hours. The temperature of the reactor is lowered to room temperature, the reactor is opened, and the filter cake is filtered. The filter cake is washed three times with N,N-dimethylformamide and anhydrous ethanol in sequence and then dried. The filter cake is transferred to a drying oven at a temperature of 55 ° C and dried to constant weight to obtain a composite modified metal powder.

[0058] S2. Preparation of modified zirconium metal powder

[0059] Weigh: 40 g of anhydrous zirconium chloride, 60 g of 2-amino-1,4-dicarboxylic acid and 400 mL of deionized water are added to a reactor and stirred. The temperature of the reactor is raised to 97°C and refluxed for 27 hours. The temperature of the reactor is lowered to 13°C, filtered, and the filter cake is immersed in anhydrous ethanol and ultrasonically dispersed for 60 minutes. Filtered, the filter cake is placed in a drying oven at a temperature of 55°C and dried to constant weight to obtain modified zirconium metal powder.

[0060] S3. Preparation of modified diatomite

[0061] Weigh: 50 g of diatomaceous earth, 10 g of tetrapropylammonium hydroxide and 500 mL of purified water were added to a reactor, stirred at room temperature for 3.5 h, filtered, the filter cake was rinsed with purified water and then dried, and the filter cake was transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain pretreated diatomaceous earth;

[0062] Ethyl orthosilicate, tetrapropylammonium hydroxide, and purified water were mixed uniformly in a ratio of 3 g:1 g:5 mL to obtain a modified solution;

[0063] The pretreated diatomaceous earth and the modified liquid were added to the reactor at a ratio of 1 g:10 mL and stirred. A heat exchange medium at a temperature of 110°C was introduced into the jacket of the reactor and stirred until the system temperature was balanced. The mixture was kept warm and stirred for 75 hours. The temperature of the reactor was lowered to room temperature and filtered. The filter cake was washed three times with purified water and then dried. The filter cake was placed in a drying oven at a temperature of 75°C and dried to constant weight. It was then transferred to a muffle furnace, the temperature of the muffle furnace was raised to 575°C, and the mixture was kept warm and calcined for 7 hours. The temperature was lowered and the material was discharged to obtain modified diatomaceous earth.

[0064] S4. Preparation of immersion dye

[0065] Sodium silicate, polydiallyldimethylammonium chloride, and purified water were mixed uniformly in a ratio of 1 g:3 g:10 mL to obtain a silicate solution;

[0066] The composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth and silicate solution were added into a reaction kettle in a dosage ratio of 3g:2g:5g:40mL and stirred evenly to obtain an impregnation dye.

[0067] S5. Prepare adsorption filler.

[0068] Mix the dye and polyurethane foam balls with a size of 5-8mm in a ratio of 7g:2.5cm 3, add it to a beaker and mix evenly, squeeze out the bubbles in the polyurethane foam ball, drain it, and then put it into the dye, repeat the dyeing operation 9 times, take the polyurethane foam ball out of the dyeing liquid and place it in a freeze dryer at a temperature of -30°C, freeze-dry it to constant weight, and then place the dry embryo obtained by freeze drying in a muffle furnace, and the muffle furnace is raised to 600°C at a rate of 1°C / min, and after keeping warm for 2 hours, it is continued to rise to 875°C at a rate of 5°C / min, and taken out after keeping warm for 3 hours, cooled and discharged to obtain an adsorption filler.

[0069] Example 3

[0070] This embodiment provides a method for preparing an adsorption filler for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0071] S1. Preparation of composite modified metal powder

[0072] Weigh: 35 g of scandium nitrate hexahydrate, 15 g of cobalt nitrate hexahydrate, 25 g of 3,3',4,4'-biphenyltetracarboxylic acid, and 500 mL of N,N,-dimethylformamide, add them to a nitrogen-protected autoclave and stir until the system is dissolved. Add 25 mL of 30 wt% hydrogen peroxide and 75 mL of pyridine to the autoclave, and pass a heat exchange medium with a temperature of 240 ° C into the jacket of the autoclave. After the pressure of the autoclave is balanced, keep warm and stir for 50 hours. The temperature of the reactor is lowered to room temperature, the reactor is opened, and the filter cake is filtered. The filter cake is washed three times with N,N-dimethylformamide and anhydrous ethanol in sequence and then dried. The filter cake is transferred to a drying oven at a temperature of 60 ° C and dried to constant weight to obtain a composite modified metal powder.

[0073] S2. Preparation of modified zirconium metal powder

[0074] Weigh: 40 g of anhydrous zirconium chloride, 60 g of 2-amino-1,4-dicarboxylic acid and 400 mL of deionized water are added to a reactor and stirred. The temperature of the reactor is raised to 100° C. and refluxed for 28 hours. The temperature of the reactor is lowered to 15° C. and filtered. The filter cake is immersed in anhydrous ethanol and ultrasonically dispersed for 60 minutes. Filtered, the filter cake is placed in a drying oven at 60° C. and dried to constant weight to obtain modified zirconium metal powder.

[0075] S3. Preparation of modified diatomite

[0076] Weigh: 50 g of diatomaceous earth, 10 g of tetrapropylammonium hydroxide and 500 mL of purified water were added to a reactor, stirred at room temperature for 4 h, filtered, the filter cake was rinsed with purified water and then dried, and the filter cake was transferred to a drying oven at 80°C and dried to constant weight to obtain pretreated diatomaceous earth;

[0077] Ethyl orthosilicate, tetrapropylammonium hydroxide, and purified water were mixed uniformly in a ratio of 3 g:1 g:5 mL to obtain a modified solution;

[0078] The pretreated diatomaceous earth and the modified liquid were added to the reactor at a ratio of 1 g:10 mL and stirred. A heat exchange medium at a temperature of 110°C was introduced into the jacket of the reactor and stirred until the system temperature was balanced. The mixture was kept warm and stirred for 78 hours. The temperature of the reactor was lowered to room temperature and filtered. The filter cake was washed three times with purified water and then dried. The filter cake was placed in a drying oven at a temperature of 80°C and dried to constant weight. It was then transferred to a muffle furnace, the temperature of the muffle furnace was raised to 600°C, the mixture was kept warm and calcined for 8 hours, and the temperature was lowered and discharged to obtain modified diatomaceous earth.

[0079] S4. Preparation of immersion dye

[0080] Sodium silicate, polydiallyldimethylammonium chloride, and purified water were mixed uniformly in a ratio of 1 g:3 g:10 mL to obtain a silicate solution;

[0081] The composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth and silicate solution were added into a reaction kettle in a dosage ratio of 3g:2g:5g:40mL and stirred evenly to obtain an impregnation dye.

[0082] S5. Prepare adsorption filler.

[0083] Mix the dye and polyurethane foam balls with a size of 5-8mm in a ratio of 7g:3cm 3 , add it to a beaker and mix evenly, squeeze out the bubbles in the polyurethane foam ball, drain it, and then put it into the dye, repeat the dyeing operation 10 times, take the polyurethane foam ball out of the dyeing liquid and place it in a freeze dryer at a temperature of -30°C, freeze-dry it to constant weight, and then place the dry embryo obtained by freeze drying in a muffle furnace, and the muffle furnace is raised to 600°C at a rate of 1°C / min, and after keeping warm for 2 hours, it is continuously raised to 900°C at a rate of 5°C / min, and taken out after keeping warm for 3 hours, cooled and discharged to obtain an adsorption filler.

[0084] Example 4

[0085] This embodiment provides a method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0086] Step 1: filtering the ethanol off-gas through a filter to remove mechanical impurities to obtain pretreated off-gas;

[0087] Step 2: The pre-treated purge gas is transported from the bottom of the methanol spray tower to the spray tower, and after methanol adsorption, the purge waste gas and methanol extract are obtained, wherein the gas-liquid ratio of the pre-treated purge gas to methanol is 1 cm 3 :3mL;

[0088] Step 3: The adsorption filler prepared in Example 1 was loaded into a tray-type distillation tower with 80 trays, forming a filler bed with a height of 8 cm on the top of the tray. One end of the feed pipe extended to above the 16th tray from the bottom up. The methanol extract was fed into the distillation tower through the feed pipe. The reflux ratio inside the distillation tower was set to 2.6 and the pressure was set to 0.6 MPa.

[0089] Step 4: A methanol pipe connected to the inside of the distillation tower is set on one side of the top of the distillation tower. One end of the methanol pipe is located inside the runoff and is above the 75th tower plate from the bottom up. After being processed by the distillation tower, the finished dimethyl ether is extracted from the top of the distillation tower, and the methanol is extracted from the methanol pipe at the top of the outside of the distillation tower and transported to the heat exchanger for cooling and heat exchange to obtain regenerated methanol. The regenerated methanol is transported to the methanol spray tower through the pipeline network for recycling.

[0090] Example 5

[0091] This embodiment provides a method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0092] Step 1: filtering the ethanol off-gas through a filter to remove mechanical impurities to obtain pretreated off-gas;

[0093] Step 2: The pre-treated purge gas is transported from the bottom of the methanol spray tower to the spray tower, and after methanol adsorption, the purge waste gas and methanol extract are obtained, wherein the gas-liquid ratio of the pre-treated purge gas to methanol is 1 cm 3 :4mL;

[0094] Step 3: The adsorption filler prepared in Example 2 was loaded into a tray-type distillation tower with 80 trays, forming a 9 cm high packing bed on top of the tray. One end of the feed pipe extended to above the 16th tray from the bottom up. The methanol extract was fed into the distillation tower through the feed pipe. The reflux ratio inside the distillation tower was set to 2.7 and the pressure was set to 0.7 MPa.

[0095] Step 4: A methanol pipe connected to the inside of the distillation tower is set on one side of the top of the distillation tower. One end of the methanol pipe is located inside the runoff and is above the 75th tower plate from the bottom up. After being processed by the distillation tower, the finished dimethyl ether is extracted from the top of the distillation tower, and the methanol is extracted from the methanol pipe at the top of the outside of the distillation tower and transported to the heat exchanger for cooling and heat exchange to obtain regenerated methanol. The regenerated methanol is transported to the methanol spray tower through the pipeline network for recycling.

[0096] Example 6

[0097] This embodiment provides a method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, comprising the following steps:

[0098] Step 1: filtering the ethanol off-gas through a filter to remove mechanical impurities to obtain pretreated off-gas;

[0099] Step 2: The pre-treated purge gas is transported from the bottom of the methanol spray tower to the spray tower, and after methanol adsorption, the purge waste gas and methanol extract are obtained, wherein the gas-liquid ratio of the pre-treated purge gas to methanol is 1 cm 3 :5mL;

[0100] Step 3: The adsorption filler prepared in Example 3 was loaded into a tray-type distillation tower with 80 trays, forming a 10 cm high filler bed on top of the tray. One end of the feed pipe extended to above the 16th tray from bottom to top. The methanol extract was fed into the distillation tower through the feed pipe. The reflux ratio inside the distillation tower was set to 2.8 and the pressure was set to 0.8 MPa.

[0101] Step 4: A methanol pipe connected to the inside of the distillation tower is set on one side of the top of the distillation tower. One end of the methanol pipe is located inside the runoff and is above the 75th tower plate from the bottom up. After being processed by the distillation tower, the finished dimethyl ether is extracted from the top of the distillation tower, and the methanol is extracted from the methanol pipe at the top of the outside of the distillation tower and transported to the heat exchanger for cooling and heat exchange to obtain regenerated methanol. The regenerated methanol is transported to the methanol spray tower through the pipeline network for recycling.

[0102] Comparative Example 1

[0103] The difference between this comparative example and Example 6 is that, in the process of preparing the adsorption filler in Example 3, cobalt nitrate hexahydrate is not added in step S1.

[0104] Comparative Example 2

[0105] The difference between this comparative example and Example 6 is that, in the process of preparing the adsorption filler in Example 3, step S2 is omitted, and modified zirconium metal powder is not added in step S4.

[0106] Comparative Example 3

[0107] The difference between this comparative example and Example 6 is that, in the process of preparing the adsorption filler in Example 3, step S3 is eliminated, and the modified diatomaceous earth in step S4 is replaced by the diatomaceous earth in step S3.

[0108] Performance testing:

[0109] The specific surface areas of the adsorption fillers used in Examples 4-6 and Comparative Examples 1-3 were measured with reference to the standard GB / T 21650.3-2011 “Determination of pore size distribution and porosity of solid materials by mercury intrusion and gas adsorption – Part 3: Analysis of micropores by gas adsorption”;

[0110] The mass fraction of dimethyl ether prepared in Examples 4-6 and Comparative Examples 1-3 and the mass fraction of methanol and water and the acidity in dimethyl ether were measured with reference to standard HG / T 3934-2007 "Dimethyl Ether". Specific test results are shown in Table 1 below.

[0111] Table 1-Performance test data of the sample

[0112]

[0113] Data Analysis:

[0114] Comparing and analyzing the data in Table 1 above, the specific surface area of ​​the adsorption filler prepared by the present invention reaches 381.4m 2 / g, the mass fraction of dimethyl ether prepared by the present invention reaches 99.8%, the mass fraction of methanol in dimethyl ether is reduced to 0.10%, and the mass fraction of water is reduced to 0.01%. All performance parameters are better than those of the comparative example;

[0115] It is explained that the present invention uses composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth and silicate solution as the impregnation liquid to impregnate polyurethane foam microspheres, and then calcines them at high temperature, which effectively increases the specific surface area of ​​the adsorption filler. By optimizing the distillation process, the separation of impurities and dimethyl ether is promoted to prepare a high-purity dimethyl ether product, reducing production energy consumption.

[0116] The above contents are merely examples and explanations of the structure of the present invention. Those skilled in the art may make various modifications or additions to the described specific embodiments or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they shall fall within the scope of protection of the present invention.

[0117] Throughout this specification, references to terms such as "one embodiment," "example," or "specific example" indicate that the specific features, structures, materials, or characteristics described in conjunction with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, schematic representations of these terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0118] The preferred embodiments of the present invention disclosed above are intended only to help illustrate the present invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the present invention to specific embodiments. Obviously, many modifications and variations are possible based on the contents of this specification. These embodiments are selected and described in detail in this specification to better explain the principles and practical applications of the present invention, thereby enabling those skilled in the art to better understand and utilize the present invention. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas, characterized in that: The following steps are involved: S1, filtering the ethanol purge gas through a filter to remove mechanical impurities to obtain pretreated purge gas; S2, transporting the pretreated purge gas from the bottom of the methanol spray tower to the spray tower, and obtaining the purge waste gas and methanol extract after methanol adsorption; S3, adding the composite modified metal powder, modified zirconium metal powder, modified diatomaceous earth, and silicate solution into a reaction kettle and stirring evenly to obtain an immersion dye, adding polyurethane foam balls into the immersion dye, squeezing out the bubbles in the polyurethane foam balls, draining, and then putting them into the immersion dye, repeating the immersion dyeing operation 8-10 times, and post-processing to obtain an adsorption filler; S4, loading an adsorption filler into a plate-type distillation tower, conveying the methanol extract from a feed pipe into the distillation tower, setting the reflux ratio inside the distillation tower to 2.6-2.8 and the pressure to 0.6-0.8 MPa; S5. After being processed in the distillation tower, the finished dimethyl ether is extracted from the top of the distillation tower, and the methanol is extracted from the methanol pipe at the top of the outside of the distillation tower and transported to the heat exchanger for cooling and heat exchange to obtain regenerated methanol. The regenerated methanol is transported to the methanol spray tower through the pipeline network for recycling.

2. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 1, characterized in that: In step S2, the gas-liquid ratio of the pre-treated purge gas to methanol is 1 cm 3 :3-5mL; in step S4, the number of plates of the distillation tower is 80, and the position of the feed pipe is above the 16th plate from bottom to top; in step S5, the position of the methanol tube is above the 75th plate from bottom to top.

3. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 1, characterized in that: In step S3, the amount ratio of the composite modified metal powder, the modified zirconium metal powder, the modified diatomaceous earth, and the silicate solution is 3g:2g:5g:40mL, the silicate solution is composed of sodium silicate, polydiallyldimethylammonium chloride and purified water in an amount ratio of 1g:3g:10mL, and the amount ratio of the impregnated dye and the polyurethane foam ball is 7g:2-3cm 3 The size of the polyurethane foam ball is 5-8 mm, and the post-treatment includes: after repeated impregnation is completed, the polyurethane foam ball is taken out from the impregnation liquid and placed in a freeze dryer, freeze-dried to constant weight, and then the dry embryo obtained by freeze drying is placed in a muffle furnace, the muffle furnace is raised to 600° C. at a rate of 1° C. / min, and after keeping warm for 2 hours, it is further raised to 850-900° C. at a rate of 5° C. / min, kept warm for 3 hours, taken out, cooled and discharged to obtain an adsorption filler.

4. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 1, characterized in that: The preparation method of the composite modified metal powder is as follows: scandium nitrate, cobalt nitrate, 3,3',4,4'-biphenyltetracarboxylic acid and N,N,-dimethylformamide are added into a nitrogen-protected high-pressure reactor and stirred until the system is dissolved, hydrogen peroxide and pyridine are added into the high-pressure reactor, a heat exchange medium with a temperature of 220-240°C is introduced into the jacket of the high-pressure reactor, after the pressure of the high-pressure reactor is balanced, the high-pressure reactor is kept warm and stirred for 40-50 hours, and the composite modified metal powder is obtained by post-treatment.

5. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 4, characterized in that: The amount ratio of scandium nitrate, cobalt nitrate, 3,3',4,4'-biphenyltetracarboxylic acid, N,N,-dimethylformamide, hydrogen peroxide and pyridine is 7g:3g:5g:100mL:5mL:15mL, the mass fraction of hydrogen peroxide is 25-30%, and the post-treatment comprises: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the reactor is opened, and the filter is filtered, the filter cake is washed with N,N-dimethylformamide and anhydrous ethanol for 3 times in sequence and then dried, the filter cake is transferred to a drying oven with a temperature of 50-60°C, and dried to constant weight to obtain a composite modified metal powder.

6. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 1, characterized in that: The preparation method of modified zirconium metal powder is as follows: anhydrous zirconium chloride, 2-amino-1,4-dicarboxylic acid and deionized water are added into a reaction kettle and stirred, the temperature of the reaction kettle is increased to 95-100° C., the reaction kettle is kept refluxed for 26-28 hours, and the modified zirconium metal powder is obtained by post-treatment.

7. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 6, characterized in that: The dosage ratio of the anhydrous zirconium chloride, 2-amino-1,4-dicarboxylic acid and deionized water is 1g:1.5g:10mL. The post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to 10-15°C, filtration is performed, the filter cake is immersed in anhydrous ethanol, ultrasonic dispersion is performed for 60 minutes, filtration is performed, the filter cake is placed in a drying oven at a temperature of 50-60°C, and dried to constant weight to obtain modified zirconium metal powder.

8. The method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 1, characterized in that: Modified diatomaceous earth is processed by the following steps: A1, adding diatomaceous earth, tetrapropylammonium hydroxide and purified water into a reaction kettle, stirring at room temperature for 3-4 hours, and post-treating to obtain pretreated diatomaceous earth; A2. Add the pretreated diatomaceous earth and the modified liquid into a reactor and stir. Pass a heat exchange medium at a temperature of 110° C. into the jacket of the reactor and stir until the system temperature is balanced. Keep the mixture warm and stir for 72-78 hours, and obtain the modified diatomaceous earth by post-treatment.

9. A method for recovering and purifying dimethyl ether from coal-to-ethanol purge gas according to claim 8, characterized in that: In step A1, the amount ratio of the diatomite, tetrapropylammonium hydroxide and purified water is 5g:1g:50mL, and the post-treatment includes: after the reaction is completed, suction filtration, rinsing the filter cake with purified water and then draining it, transferring the filter cake to a drying oven at a temperature of 70-80°C, and drying it to constant weight to obtain pretreated diatomite; in step A2, the amount ratio of the pretreated diatomite and the modifying liquid is 1g:10mL, and the modifying liquid is composed of ethyl orthosilicate, tetrapropylammonium hydroxide and purified water in an amount ratio of 3g:1g:5mL, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration, washing the filter cake with purified water 3 times and then draining it, placing the filter cake in a drying oven at a temperature of 70-80°C and drying it to constant weight, and then transferring it to a muffle furnace, the temperature of the muffle furnace is raised to 550-600°C, and the muffle furnace is kept warm and calcined for 6-8h, and the temperature is lowered and discharged to obtain modified diatomite.

Citation Information

Patent Citations

  • Production process for energy-saving environment-friendly methanol dehydration joint production of combustion extractive dimethyl ether

    CN101492349A

  • Method for preparing dimethyl ether with high purity by syngas one-step method

    CN101607873A

  • Crude alcohol purification and recovery process based on coal-based fuel ethanol

    CN118561660A

  • Production method of non-convertible combined methanol and dimethyl ether from coke oven gas

    CN1876614A

Cited By

  • Method for recovering dimethyl ether from dimethyl ether purge gas

    CN119504376A