Synthetic method of water-based acrylic resin emulsion

By mixing acrylic acid, pH buffer and emulsifier in the stirring device, combining the use of deionized water and ammonium sulfate, a high-efficiency aqueous acrylic resin emulsion is formed, and the VOC reduction is reduced through the secondary dispersion, the high VOC in the prior art is solved. The problem is to achieve a balance between coating performance and environmental protection, and improve the film formation effect and weather resistance of the finished product.

CN118955782APending Publication Date: 2024-11-15JIANGXI ZHEWEI NEW MATERIALS TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410316179.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing aqueous acrylic resin has a high VOC content, which is difficult to meet the user's balance of coating performance and environmental protection, and there are potential harms to the human body and the environment when used.

Method used

Using an aqueous acrylic resin emulsion synthesis method, the pre-emulsion is generated by mixing acrylic acid, pH buffer and emulsifier in a stirring device, and deionized water and ammonium sulfate are added as initiators to control the temperature and The stirring speed is used to form an efficient aqueous acrylic resin emulsion, which is further mixed by the secondary dispersion to reduce the VOC content.

Benefits of technology

Improve reaction efficiency, increase cross-link density, and make the finished product have good film formation effect, high gloss, good hardness, excellent water resistance and chemical resistance. At the same time, it reduces VOC content and enhances the melting with powder. It is suitable for use. In the fields of industrial and civil coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004748982470000061
    Figure BDA0004748982470000061
  • Figure BDA0004748982470000091
    Figure BDA0004748982470000091
Patent Text Reader

Abstract

The invention discloses a water-based acrylic resin emulsion synthesis method, which comprises: adding acrylic acid and water into a first mixing container according to a formula ratio, stirring the mixed solution by using a stirring device at a stirring speed of 150-200 rpm for 1-2 min, adding a pH buffer agent and an emulsifier, and stirring for 2-3 min. According to the invention, acrylic acid, a pH buffer agent, an emulsifier and water are mixed to prepare a pre-emulsion, and meanwhile, bottom water is prepared in a second mixing container and then mixed, so that the reaction efficiency can be improved, and the compounding mode can increase the crosslinking density, so that when a finished product is used, the film forming effect is good, the use amount of a film forming auxiliary agent is reduced, the product is easy to polish, and the glossiness is relatively good; in the preparation process, a PH buffering agent is adopted for multiple times, PH value control is carried out on all the steps, the PH value in the emulsion reaction and mixing process is kept stable, the impurity content in the synthesis process is low, and the polymerization reaction is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based coating synthesis methods, and in particular to a method for synthesizing a water-based acrylic resin emulsion. Background Art

[0002] Water-based acrylic resins include acrylic resin emulsions, acrylic resin aqueous dispersions and acrylic resin aqueous solutions. The emulsions are mainly synthesized by emulsifying oily olefin monomers in water under the initiation of water-based free radical initiators, while the resin aqueous dispersions are synthesized through different processes such as free radical solution polymerization or step solution polymerization. They are mainly used as base materials for latex paints and have an important application in the architectural coatings market. Their applications are still expanding. In recent years, the development and application of acrylic resin aqueous dispersions have attracted increasing attention, and their applications in the fields of industrial coatings and civil coatings have been continuously expanding.

[0003] In the prior art, commonly used water-dilutable acrylic resins refer to water-based acrylic resins synthesized by solution polymerization and then phase inversion. They still have a relatively high VOC and are mainly used as the hydroxyl component of amino stoving varnishes. With the development of the times, people have higher demands for health and environmental protection. The preparation requirements for water-based acrylic resin emulsions are also pursuing a balance between coating performance and environmental protection, meeting user needs while reducing harm to the human body and the environment. To this end, we propose a method for synthesizing a water-based acrylic resin emulsion to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to solve the problems existing in the prior art and to propose a method for synthesizing an aqueous acrylic resin emulsion.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for synthesizing a water-based acrylic resin emulsion, characterized in that the synthesis method is:

[0007] S1. Add acrylic acid and water into a first mixing container according to the formula ratio, and then stir the mixture with a stirring device at a stirring speed of 150-200 rpm. After stirring for 1-2 minutes, add a pH buffer and an emulsifier, and stir for another 2-3 minutes. Then, add methyl methacrylate while the stirring device is running, and then increase the stirring speed to 300-350 rpm and continue stirring for 30 minutes to obtain a pre-emulsion;

[0008] S2, taking out a portion of the pre-emulsion as a reaction and adding the seed emulsion dropwise;

[0009] S3, adding a portion of ammonium sulfate as an initiator to the pre-emulsion, and continuing to stir for 15 minutes while maintaining the rotation speed;

[0010] S4, first add deionized water, pH buffer and emulsifier as bottom water into the second mixing container, then stir and heat to 92°C;

[0011] S5, adding the seed emulsion taken out in S2 into the second mixing container, and adding the remaining ammonium sulfate as an initiator into the bottom water and stirring for 10 to 15 minutes, observing that the bottom water turns blue, and continuing to stir for 1 to 2 minutes;

[0012] S6, continuously dripping the pre-emulsion prepared in S1 into the second mixing container, and controlling the reaction temperature at 85° C., and keeping the temperature for 1 hour after the dripping is completed;

[0013] S7, after cooling the finished product, remove impurities by filtering to obtain the finished product.

[0014] Preferably, it is made from the following raw materials in the following mass ratio:

[0015] Deionized water 57-59%, methyl methacrylate 7-20%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%, and the rest is water;

[0016] Preferably, the synthesis of the aqueous acrylic resin emulsion further includes a secondary dispersion, and the secondary dispersion is made of raw materials with the following mass ratio:

[0017] Propylene glycol butyl ether 3.3-3.6%, xylene 5.2-5.4%, methyl methacrylate 22-24.5%, butyl acrylate 13.5-14.2%, hydroxyethyl methacrylate 13-13.6% and benzoyl peroxide 1.2-1.75%, acrylic acid 0.7-1.2%, dimethylethanolamine 1.6-1.75%, and the rest is water.

[0018] Preferably, it is made from the following raw materials in the following mass ratio:

[0019] Deionized water 57-59%, styrene 20-22%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%.

[0020] Preferably, it is made from the following raw materials in the following mass ratio:

[0021] Deionized water 57-59%, methyl methacrylate 10-12%, styrene 8-11%, polymerizable silane 0.15-0.22%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%.

[0022] Preferably, the synthesis method of the secondary dispersion is:

[0023] (1) Mix propylene glycol butyl ether and xylene, stir, and heat to 135° C. as a solvent;

[0024] (2) 18-20.5% of methyl methacrylate, 9.5-10% of butyl acrylate, 9.2-1.45% of benzoyl peroxide, and 8-8.8% of hydroxyethyl methacrylate are mixed as group one, and then group one is added dropwise to the solution for 2.5 hours;

[0025] (3) At the same time, the remaining methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, and benzoyl peroxide are mixed to prepare group 2;

[0026] (4) After the addition of group 1 is completed, group 2 is added to the solvent for 1.5 hours. After the addition is completed, keep warm for 3 hours;

[0027] (5) After the heat preservation is completed, the mixed solvent is cooled to below 100° C., dimethylethanolamine is added as a neutralizing agent and stirred at a stirring speed of 600 to 850 rpm, and water is added and dispersed at a high speed after stirring for 2 to 3 minutes.

[0028] 4. A method for synthesizing a water-based acrylic resin emulsion according to claims 2 and 3, characterized in that the method for synthesizing the water-based acrylic resin emulsion comprises mixing the finished product with a secondary dispersion and fully stirring to obtain a secondary dispersed water-based acrylic resin emulsion.

[0029] Preferably, after the temperature of the finished product drops below 40° C., the pH value of the finished product is detected, and then the pH buffer is added again to adjust the pH value to 7 to 7.5.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The present invention adopts acrylic acid, pH buffer and emulsifier and water to mix to form pre-emulsion, and prepares base water in a second mixing container before mixing, which can improve the reaction efficiency, and this compounding method can increase the cross-linking density, so that the finished product has good film-forming effect when used, reduces the amount of film-forming aid, is easy to polish and has good gloss.

[0032] 2. The present invention, by providing a secondary dispersion, can effectively reduce the VOC content after the finished product is mixed with the secondary dispersion, and can increase the hardness building speed of the water-based acrylic resin emulsion when used, and can be transparent after molding, and when it is matched with powder for solid color painting, it has good compatibility with the powder and does not become rough.

[0033] 3. The present invention uses pH buffers multiple times during the preparation process to control the pH value of each step. The pH value remains stable during the emulsion reaction and mixing process, the impurity content is low during the synthesis process, the polymerization reaction is stable, the coating has high gloss after film formation, good hardness, water resistance, good fullness, and good weather resistance and chemical resistance. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0035] Embodiment 1, a method for synthesizing a water-based acrylic resin emulsion, the synthesis method is:

[0036] S1. Add acrylic acid and water into a first mixing container according to the formula ratio, and then stir the mixture with a stirring device at a stirring speed of 150-200 rpm. After stirring for 1-2 minutes, add a pH buffer and an emulsifier, and stir for another 2-3 minutes. Then, add methyl methacrylate while the stirring device is running, and then increase the stirring speed to 300-350 rpm and continue stirring for 30 minutes to obtain a pre-emulsion;

[0037] S2, taking out a portion of the pre-emulsion as a reaction and adding the seed emulsion dropwise;

[0038] S3, adding a portion of ammonium sulfate as an initiator to the pre-emulsion, and continuing to stir for 15 minutes while maintaining the rotation speed;

[0039] S4, first add deionized water, pH buffer and emulsifier as bottom water into the second mixing container, then stir and heat to 92°C;

[0040] S5, adding the seed emulsion taken out in S2 into the second mixing container, and adding the remaining ammonium sulfate as an initiator into the bottom water and stirring for 10 to 15 minutes, observing that the bottom water turns blue, and continuing to stir for 1 to 2 minutes;

[0041] S6, continuously dripping the pre-emulsion prepared in S1 into the second mixing container, and controlling the reaction temperature at 85° C., and keeping the temperature for 1 hour after the dripping is completed;

[0042] S7, after cooling the finished product, remove impurities by filtering to obtain the finished product.

[0043] The aqueous acrylic resin emulsion is synthesized from the following raw materials in the following mass ratio:

[0044] Deionized water 57-59%, methyl methacrylate 7-20%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%, and the rest is water. This ratio is pure acrylic emulsion;

[0045] Table 1

[0046] raw material Proportion Deionized water 58 Methyl Methacrylate 18.2 Butyl acrylate 10 2-Ethylhexyl acrylate 10 acrylic acid 0.65 Ammonium Persulfate 0.55 Emulsifier 0.8 ammonia 0.6 pH buffer 1.2

[0047] In this configuration, the average particle size of the emulsion measured in the test is 48.60nm, and it is highly densely dispersed. The conversion rate of the emulsion is 82%-93%. It is mainly used in the civil and textile fields, but mainly for non-long-term contact items. Generally speaking, it is harmless to human contact, but there are still risks due to VOC or other impurities.

[0048] In Example 2, the synthesis of the aqueous acrylic resin emulsion also includes a secondary dispersion, and the secondary dispersion is made of the following raw materials in the following mass ratio:

[0049] Propylene glycol butyl ether 3.3-3.6%, xylene 5.2-5.4%, methyl methacrylate 22-24.5%, butyl acrylate 13.5-14.2%, hydroxyethyl methacrylate 13-13.6% and benzoyl peroxide 1.2-1.75%, acrylic acid 0.7-1.2%, dimethylethanolamine 1.6-1.75%, and the rest is water.

[0050] Table 2

[0051]

[0052] In this configuration, the average particle size of the emulsion measured after testing is 45.30nm, and it is highly densely dispersed, and the conversion rate of the emulsion is 76%-88%. Due to the use of secondary dispersion, the emulsion particles are smaller and more delicate, but the emulsion conversion rate is reduced, and the production cost becomes higher, but the VOC content is further reduced, and it has a more obvious advantage in harmlessness, especially when it is matched with powder for solid color painting, it has good compatibility with the powder and does not become coarse.

[0053] Example 3 is made from the following raw materials in the following mass ratio:

[0054] Deionized water 57-59%, styrene 20-22%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%, this ratio is styrene emulsion.

[0055] Table 3

[0056] raw material Proportion Deionized water 58 Styrene 19.6 Butyl acrylate 10 2-Ethylhexyl acrylate 8 acrylic acid 0.55 Ammonium Persulfate 0.8 Emulsifier 1 ammonia 0.85 pH buffer 1.2

[0057] In this configuration, the average particle size of the emulsion measured in the test is 52.40nm, and the conversion rate of the emulsion is 84%-95%. This configuration is a silicone acrylic emulsion formula with low surface energy and low pollution resistance, and is more focused on use in the construction field.

[0058] Example 4 is prepared from the following raw materials in the following mass ratio:

[0059] The composition includes 57-59% deionized water, 10-12% methyl methacrylate, 8-11% styrene, 0.15-0.22% polymerizable silane, 9.5-10.5% butyl acrylate, 7-12% isooctyl acrylate, 0.5-0.7% acrylic acid, 0.3-0.75% ammonium persulfate, 0.8-1% emulsifier, 0.5-1.2% ammonia water and 1.5-2% pH buffer. This is a silicone-acrylic emulsion.

[0060] Table 4

[0061] raw material Proportion Deionized water 58 Methyl Methacrylate 8 Styrene 10 Butyl acrylate 10 Polymerizable silane 0.3 2-Ethylhexyl acrylate 9.6 acrylic acid 0.6 Ammonium Persulfate 0.55 Emulsifier 0.9 ammonia 0.55 pH buffer 1.5

[0062] In this configuration, the average particle size of the emulsion measured by the test is 55.54nm, the conversion rate of the emulsion is 90%-95%, and this configuration is a styrene emulsion formula.

[0063] Comparative Example

[0064] Anionic surfactant 0.3-0.9%, nonionic surfactant 0.3-1.2%, methacrylic acid, methyl ester monomer 6.2-21.03%, butyl acrylate monomer 8.97-23.8%, crosslinking monomer 0.92-

[0065] 1.63%, fluorine monomer 0.62-1.61%, silicon monomer 0.3-1.54%, initiator 0.09-0.21%, the balance is water

[0066] Resin emulsion performance indicators and test results

[0067] Comparison table

[0068]

[0069] When the water-based acrylic resin emulsion synthesis method is adopted, after the emulsion is mixed into the emulsion, as compared with Example 1, the diameter of the emulsion particles in Example 1 is about 73% of that in the comparative example, and the particle diameter is reduced by 27%. The volume of the emulsion particles in Example 1 is only 38% of that in the comparative example. In general, the smaller the emulsion particles of the water-based paint thickener, the better the thickening efficiency. This is because the surface area in contact with the emulsion increases, the smaller the particle size, the greater the viscosity, and the size of the emulsion particles has a greater impact on the thickener. It will have a significant improvement in subsequent actual use, and the fine particles can better fill the gaps and have a higher bonding effect after curing. Secondly, the solid content is increased. While the particle size is significantly reduced, the proportion of the solidified content is increased, so that the proportion of the effective ingredients of the water-based acrylic resin emulsion is higher, and the overall amount required during use is reduced. Secondly, the conversion rate is increased by about 10%, which increases the output, thereby reducing impurities in the production process (which will be affected by the quality of raw materials), improving the purity of the product itself, and improving the output and quality.

[0070] Preferably, the synthesis method of the secondary dispersion is:

[0071] (1) Mix propylene glycol butyl ether and xylene, stir, and heat to 135° C. as a solvent;

[0072] (2) 18-20.5% of methyl methacrylate, 9.5-10% of butyl acrylate, 9.2-1.45% of benzoyl peroxide, and 8-8.8% of hydroxyethyl methacrylate are mixed as group one, and then group one is added dropwise to the solution for 2.5 hours;

[0073] (3) At the same time, the remaining methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, and benzoyl peroxide are mixed to prepare group 2;

[0074] (4) After the addition of group 1 is completed, group 2 is added to the solvent for 1.5 hours. After the addition is completed, keep warm for 3 hours;

[0075] (5) After the heat preservation is completed, the mixed solvent is cooled to below 100° C., dimethylethanolamine is added as a neutralizing agent and stirred at a stirring speed of 600 to 850 rpm, and water is added and dispersed at a high speed after stirring for 2 to 3 minutes.

[0076] Furthermore, the method for synthesizing the water-based acrylic resin emulsion is to mix the finished product with the secondary dispersion and fully stir to obtain the secondary dispersed water-based acrylic resin emulsion. The secondary dispersed water-based acrylic resin emulsion prepared by mixing the finished product with the secondary dispersion can further reduce the VOC content, not only shorten the hardness building time, but also ensure the gloss after film formation, which is closer to the balance point between coating performance and environmental protection.

[0077] Furthermore, after the temperature of the finished product drops below 40° C., the pH value of the finished product is detected, and then the pH buffer is added again to adjust the pH value to 7-7.5.

[0078] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for synthesizing an aqueous acrylic resin emulsion, It is characterized in that The synthesis method is: S1. Add acrylic acid and water into a first mixing container according to the formula ratio, and then stir the mixture with a stirring device at a stirring speed of 150-200 rpm. After stirring for 1-2 minutes, add a pH buffer and an emulsifier, and stir for another 2-3 minutes. Then, add methyl methacrylate while the stirring device is running, and then increase the stirring speed to 300-350 rpm and continue stirring for 30 minutes to obtain a pre-emulsion; S2, taking out a portion of the pre-emulsion as a reaction and adding the seed emulsion dropwise; S3, adding a portion of ammonium sulfate as an initiator to the pre-emulsion, and continuing to stir for 15 minutes while maintaining the rotation speed; S4, first add deionized water, pH buffer and emulsifier as bottom water into the second mixing container, then stir and heat to 92°C; S5, adding the seed emulsion taken out in S2 into the second mixing container, and adding the remaining ammonium sulfate as an initiator into the bottom water and stirring for 10 to 15 minutes, observing that the bottom water turns blue, and continuing to stir for 1 to 2 minutes; S6, continuously dripping the pre-emulsion prepared in S1 into the second mixing container, and controlling the reaction temperature at 85° C., and keeping the temperature for 1 hour after the dripping is completed; S7, after cooling the finished product, remove impurities by filtering to obtain the finished product.

2. A method for synthesizing an aqueous acrylic resin emulsion according to claim 1, It is characterized in that Made of raw materials with the following mass ratio: Deionized water 57-59%, methyl methacrylate 7-20%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%, and the rest is water.

3. A method for synthesizing an aqueous acrylic resin emulsion according to claim 2, It is characterized in that The synthesis of the aqueous acrylic resin emulsion also includes a secondary dispersion, which is made of the following raw materials in the following mass ratio: Propylene glycol butyl ether 3.3-3.6%, xylene 5.2-5.4%, methyl methacrylate 22-24.5%, butyl acrylate 13.5-14.2%, hydroxyethyl methacrylate 13-13.6% and benzoyl peroxide 1.2-1.75%, acrylic acid 0.7-1.2%, dimethylethanolamine 1.6-1.75%, and the rest is water.

4. A method for synthesizing an aqueous acrylic resin emulsion according to claim 1, It is characterized in that Made of raw materials with the following mass ratio: Deionized water 57-59%, styrene 20-22%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%.

5. A method for synthesizing an aqueous acrylic resin emulsion according to claim 1, It is characterized in that Made of raw materials with the following mass ratio: Deionized water 57-59%, methyl methacrylate 10-12%, styrene 8-11%, polymerizable silane 0.15-0.22%, butyl acrylate 9.5-10.5%, isooctyl acrylate 7-12%, acrylic acid 0.5-0.7%, ammonium persulfate 0.3-0.75%, emulsifier 0.8-1%, ammonia water 0.5-1.2%, pH buffer 1.5-2%.

6. A method for synthesizing an aqueous acrylic resin emulsion according to claim 3, It is characterized in that The synthesis method of the secondary dispersion is: (1) Mix propylene glycol butyl ether and xylene, stir, and heat to 135° C. as a solvent; (2) 18-20.5% of methyl methacrylate, 9.5-10% of butyl acrylate, 9.2-1.45% of benzoyl peroxide, and 8-8.8% of hydroxyethyl methacrylate are mixed as group one, and then group one is added dropwise to the solution for 2.5 hours; (3) At the same time, the remaining methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, and benzoyl peroxide are mixed to prepare group 2; (4) After the addition of group 1 is completed, group 2 is added to the solvent for 1.5 hours. After the addition is completed, keep warm for 3 hours; (5) After the heat preservation is completed, the mixed solvent is cooled to below 100° C., dimethylethanolamine is added as a neutralizing agent and stirred at a stirring speed of 600 to 850 rpm, and water is added and dispersed at a high speed after stirring for 2 to 3 minutes.

7. A method for synthesizing an aqueous acrylic resin emulsion according to any one of claims 2 or 3, It is characterized in that The method for synthesizing the water-based acrylic resin emulsion comprises mixing the finished product with a secondary dispersion and fully stirring the mixture to obtain a secondary dispersed water-based acrylic resin emulsion.

8. A method for synthesizing an aqueous acrylic resin emulsion according to claim 1, It is characterized in that After the temperature of the finished product drops below 40° C., the pH value of the finished product is detected, and then the pH buffer is added again to adjust the pH value to 7-7.5.

Citation Information

Patent Citations

  • Hydroxyl-containing polyacrylate secondary water dispersion and preparation method thereof

    CN109608575A

  • Water-based plastic substitute and preparation method thereof

    CN113249063A

  • High-permeability hydroxyl acrylic emulsion as well as preparation method and application thereof

    CN117510707A

  • Copolymer latex for water-based paint

    JP1999035872A