Irradiation crosslinking sensitizer as well as preparation method and application thereof
High boiling point irradiation crosslinking sensitizer is prepared by reacting the compound of carbon-carbon double bond and silicon-hydrogen bond, which solves the problem of volatility and self-polymerization of existing sensitizers in high-temperature environments and improves fluorine-containing polymerization The cross-linking effect and mechanical properties of objects are suitable for applications in aerospace and other fields.
Patent Information
- Application Number
- CN202410986633.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing radiation crosslinking sensitizers are easy to volatilize, self-polymerize and have a low boiling point in high-temperature processing environments, and cannot effectively improve the crosslinking effect of fluoropolymers, affecting their application in aerospace and other fields.
By reacting compounds containing multiple carbon-carbon double bonds with silicone hydrogen bonds, an irradiation crosslinking sensitizer with high boiling point and good thermal stability is prepared, and an inhibitor and a catalyst are added during the preparation process. Reaction conditions to improve crosslinking effect.
The prepared irradiation crosslinking sensitizer has high boiling point, good thermal stability and assisted crosslinking effect, which reduces the degradation of molecular chains, is suitable for processing and modification of fluoropolymers, and improves its mechanical properties and It has low processing performance and low production cost, making it suitable for large-scale industrial production.
Smart Images

Figure CN118955909A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material processing aids, and in particular to a radiation cross-linking sensitizer and a preparation method and application thereof. Background Art
[0002] Fluoropolymers contain carbon-carbon bonds and carbon-fluorine bonds (the special electronic structure of the fluorine element gives it high electronegativity, low polarizability and small van der Waals radius). Compared with fluorine-free polymers, they have better thermal stability and weather resistance, and lower friction coefficient and surface energy. They are widely used in many fields such as construction, automobiles, aerospace, textiles, energy, microelectronics, biomedicine, etc. Fluoropolymers need to be cross-linked under irradiation to further improve their thermal stability, mechanical properties, dielectric properties and other properties, so that they can be better used in harsh environmental fields such as aerospace. However, when fluorine-containing polymers are cross-linked by radiation, the molecular chain will also degrade, which will affect the cross-linking effect of the polymer. Therefore, it is necessary to add a suitable radiation cross-linking sensitizer to improve the cross-linking effect and reduce the degradation of the molecular chain. At present, common radiation cross-linking sensitizers include triallyl isocyanurate (TAIC), trimethylallyl isocyanate (TMAIC), triallyl cyanurate (TAC), etc. The boiling points of these radiation cross-linking sensitizers are all lower than 200°C, which cannot meet the high-temperature processing environment of fluorinated polymers. They are easy to volatilize (produce a large amount of toxic fumes) and self-polymerize during the processing, and cannot achieve the ideal cross-linking effect.
[0003] Therefore, it is of great significance to develop a radiation cross-linking sensitizer with high boiling point, good thermal stability, good cross-linking effect and low production cost. Summary of the invention
[0004] The purpose of the present invention is to provide a radiation cross-linking sensitizer and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention is:
[0006] A radiation cross-linking sensitizer is obtained by reacting a compound containing multiple carbon-carbon double bonds and silicone oil containing silicon-hydrogen bonds; the compound containing multiple carbon-carbon double bonds is at least one of triallyl isocyanurate (TAIC), trimethallyl isocyanate (TMAIC) and triallyl cyanurate (TAC).
[0007] Preferably, the molar ratio of carbon-carbon double bonds in the compound containing multiple carbon-carbon double bonds to silicon-hydrogen bonds in the silicone oil containing silicon-hydrogen bonds is 1 to 6:1.
[0008] Preferably, the hydrogen content of the silicone oil containing silicon-hydrogen bonds is less than 2 wt %.
[0009] A method for preparing the radiation cross-linking sensitizer as described above comprises the following steps:
[0010] A compound containing multiple carbon-carbon double bonds, an inhibitor and a catalyst are dispersed in a solvent, and then silicone oil containing silicon-hydrogen bonds is added and the temperature is raised to react, thereby obtaining a radiation cross-linking sensitizer.
[0011] Preferably, the inhibitor is used in an amount of 0.2% to 1.5% by weight of the silicone oil containing silicon-hydrogen bonds.
[0012] Preferably, the inhibitor is at least one of 1-ethynylcyclohexanol, 2-vinylisopropanol, and 1-ethynylcyclopentanol.
[0013] Preferably, the amount of the catalyst used is 0.2% to 2% by weight of the silicone oil containing silicon-hydrogen bonds.
[0014] Preferably, the catalyst is at least one of a Custer catalyst, platinum phosphate, and chloroplatinic acid.
[0015] Preferably, the solvent is at least one of toluene and xylene.
[0016] Preferably, the reaction is carried out at a temperature of 70°C to 110°C and the reaction time is 2h to 10h.
[0017] More preferably, the reaction is carried out at a temperature of 90° C. to 110° C., and the reaction time is 2 h to 4 h.
[0018] Preferably, the reaction is carried out at a stirring speed of 80 r / min to 180 r / min.
[0019] More preferably, the reaction is carried out at a stirring speed of 100 r / min to 150 r / min.
[0020] Preferably, after the reaction is completed, the product is further subjected to ethanol extraction and column chromatography purification.
[0021] A fluorine-containing polymer product comprises the above-mentioned radiation cross-linking sensitizer.
[0022] Preferably, the weight ratio of the fluorinated polymer to the radiation cross-linking sensitizer in the fluorinated polymer product is 100:0.05-20.
[0023] A method for preparing the fluorine-containing polymer article as described above comprises the following steps:
[0024] The fluorine-containing polymer and the radiation cross-linking sensitizer are mixed and subjected to extrusion molding or injection molding, and then subjected to radiation cross-linking to obtain the fluorine-containing polymer product.
[0025] Preferably, the radiation cross-linking is performed at a radiation dose of 10 Mrad to 120 Mrad.
[0026] Preferably, the product is annealed after the radiation cross-linking is completed.
[0027] Preferably, the annealing is performed at a temperature of 100° C. to 130° C., and the annealing time is 1 h to 3 h.
[0028] The beneficial effects of the present invention are as follows: the radiation cross-linking sensitizer of the present invention has the advantages of high boiling point, good thermal stability, good cross-linking auxiliary effect, low production cost, etc., can effectively improve the cross-linking effect of fluorine-containing polymers and reduce the degradation of molecular chains, and its preparation method is simple to operate and the reaction conditions are mild, and it is suitable for large-scale industrial production and application.
[0029] Specifically:
[0030] 1) The radiation cross-linking sensitizer of the present invention is a long-chain macromolecule, and the cross-linked network structure formed by the sensitizer in the fluorine-containing polymer can effectively improve the mechanical properties of the fluorine-containing polymer;
[0031] 2) The radiation cross-linking sensitizer of the present invention is in liquid state at room temperature, has a boiling point higher than 250°C, has excellent thermal stability, and is not prone to self-polymerization, and can meet the processing modification requirements of most fluorine-containing polymers. During the processing, the liquid radiation cross-linking sensitizer can also act as a plasticizer for the fluorine-containing polymer, thereby effectively improving the processing properties of the fluorine-containing polymer;
[0032] 3) The preparation process of the radiation cross-linking sensitizer of the present invention is simple to operate, low in cost, and has mild reaction conditions. It can be prepared quickly and in large quantities, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the FTIR graph of the radiation cross-linking sensitizer in Example 1.
[0034] Figure 2 This is the FTIR graph of the radiation cross-linking sensitizer in Example 2.
[0035] Figure 3 This is the FTIR graph of the radiation cross-linking sensitizer in Example 3.
[0036] Figure 4 This is the FTIR graph of the radiation cross-linking sensitizer in Example 4.
[0037] Figure 5 This is the FTIR graph of the radiation cross-linking sensitizer in Example 5.
[0038] Figure 6This is the FTIR graph of the radiation cross-linking sensitizer in Example 6.
[0039] Figure 7 This is the FTIR graph of the radiation cross-linking sensitizer in Example 7. DETAILED DESCRIPTION
[0040] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0041] Embodiment 1:
[0042] A radiation cross-linking sensitizer, the preparation method of which is as follows:
[0043] Mix 20g of triallyl isocyanurate (TAIC) and 0.2g of 1-ethynylcyclohexanol and stir evenly, then add 0.2g of Custer catalyst (PT-5000 of Guangzhou Xiyi Chemical Co., Ltd.) and 60mL of toluene and stir evenly, then add 10g of silicon-hydrogen bond-containing silicone oil with a hydrogen content of 0.8wt% (DFH-08 of Guangzhou Jibisheng Technology Industrial Co., Ltd.) and stir evenly, then heat to 100°C and stir to react for 4h at a stirring speed of 100r / min, cool naturally to room temperature, and then use ethanol extraction to remove unreacted triallyl isocyanurate and toluene in the product, and then use silica gel column for column chromatography to purify and remove the Custer catalyst. The eluent used for column chromatography is methanol, and then perform reduced pressure distillation to obtain the radiation cross-linking sensitizer.
[0044] The Fourier transform infrared spectrum (FTIR) of the radiation cross-linking sensitizer in this example is as follows: Figure 1 shown.
[0045] Depend on Figure 1 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0046] According to the test, the boiling point of the radiation cross-linking sensitizer in this embodiment is 304°C.
[0047] A fluorine-containing polymer product (standard sample), the preparation method of which is as follows:
[0048] The fluoropolymer EP-521 of Shanghai Jinfu Chemical Technology Co., Ltd. and the radiation cross-linking sensitizer in this embodiment were added to a twin-screw extruder in a weight ratio of 100:4 for extrusion granulation. During the extrusion process, the temperatures of barrel zone 1, barrel zone 2, barrel zone 3, barrel zone 4, barrel zone 5, barrel zone 6, barrel zone 7, barrel zone 8 and die zone of the extruder were set to 260°C, 265°C, 265°C, 265°C, 270°C, 275°C, 280°C, 280°C and 285°C, respectively, the speed of the main screw was set to 120rpm, and the speed of the feeder screw was set to 30rpm. The extruded pellets were placed in a flat vulcanizer at 280°C and pressed into standard strips, and the strips were then placed under an irradiation dose of 15Mrad for 5 minutes of electron irradiation to obtain fluoropolymer products.
[0049] Embodiment 2:
[0050] A radiation cross-linking sensitizer is exactly the same as Example 1 except that the amount of triallyl isocyanurate is adjusted from "20g" to "30g" during preparation.
[0051] The FTIR image of the radiation cross-linking sensitizer in this example is as follows: Figure 2 shown.
[0052] Depend on Figure 2 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0053] According to the test, the boiling point of the radiation cross-linking sensitizer in this embodiment is 318° C., which is higher than that of the radiation cross-linking sensitizer in Example 1. The reason is that the increase in the amount of TAIC promotes its reaction with the silicone oil containing silicon-hydrogen bonds.
[0054] A fluorine-containing polymer product is identical to Example 1 except that during preparation, the weight of the radiation cross-linking sensitizer is replaced by the radiation cross-linking sensitizer in this example.
[0055] Embodiment 3:
[0056] A radiation cross-linking sensitizer is exactly the same as Example 1 except that the amount of triallyl isocyanurate is adjusted from "20g" to "10g" during preparation.
[0057] The FTIR image of the radiation cross-linking sensitizer in this example is as follows: Figure 3 shown.
[0058] Depend on Figure 3 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0059] According to the test, the boiling point of the radiation cross-linking sensitizer in this embodiment is 293° C., which is lower than that of the radiation cross-linking sensitizer in Example 1. The reason is that the amount of TAIC used is reduced, which weakens its reaction with the silicone oil containing silicon-hydrogen bonds.
[0060] A fluorine-containing polymer product is identical to Example 1 except that during preparation, the weight of the radiation cross-linking sensitizer is replaced by the radiation cross-linking sensitizer in this example.
[0061] Embodiment 4:
[0062] A radiation cross-linking sensitizer is prepared in the same manner as in Example 1 except that the amount of the Custer catalyst is adjusted from "0.2g" to "0.4g".
[0063] The FTIR image of the radiation cross-linking sensitizer in this example is as follows: Figure 4 shown.
[0064] Depend on Figure 4 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0065] According to the test, the boiling point of the radiation cross-linking sensitizer in this embodiment is 313° C., which is higher than that in Example 1. The reason is that the increase in the amount of the Custer catalyst promotes the reaction between TAIC and the silicone oil containing silicon-hydrogen bonds.
[0066] A fluorine-containing polymer product is identical to Example 1 except that during preparation, the weight of the radiation cross-linking sensitizer is replaced by the radiation cross-linking sensitizer in this example.
[0067] Embodiment 5:
[0068] A radiation cross-linking sensitizer is prepared in the same manner as in Example 1 except that the amount of 1-ethynylcyclohexanol used is adjusted from "0.2 g" to "0.4 g".
[0069] The FTIR image of the radiation cross-linking sensitizer in this example is as follows: Figure 5 shown.
[0070] Depend on Figure 5 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0071] After testing, the boiling point of the radiation cross-linking sensitizer in this embodiment is 302°C, which is close to the boiling point of the radiation cross-linking sensitizer in Example 1, indicating that 1-ethynyl cyclohexanol is basically completely volatilized during the heating process and will not affect the boiling point of the radiation cross-linking sensitizer.
[0072] A fluorine-containing polymer product is identical to Example 1 except that during preparation, the weight of the radiation cross-linking sensitizer is replaced by the radiation cross-linking sensitizer in this example.
[0073] Embodiment 6:
[0074] A radiation cross-linking sensitizer is prepared in the same manner as in Example 1 except that the stirring speed is adjusted from "100 r / min" to "180 r / min".
[0075] The FTIR image of the radiation cross-linking sensitizer in this example is as follows: Figure 6 shown.
[0076] Depend on Figure 6 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0077] According to the test, the boiling point of the radiation cross-linking sensitizer in this embodiment is 295° C., which is lower than that of the radiation cross-linking sensitizer in Example 1. The reason is that the stirring speed is too fast, which weakens the reaction between TAIC and the silicone oil containing silicon-hydrogen bonds.
[0078] A fluorine-containing polymer product is identical to Example 1 except that during preparation, the weight of the radiation cross-linking sensitizer is replaced by the radiation cross-linking sensitizer in this example.
[0079] Embodiment 7:
[0080] A radiation cross-linking sensitizer is completely the same as Example 1 except that the reaction time is adjusted from "4h" to "7h" during preparation.
[0081] The FTIR image of the radiation cross-linking sensitizer in this example is as follows: Figure 7 shown.
[0082] Depend on Figure 7 It can be seen that TAIC successfully reacts with silicone oil containing silicon-hydrogen bonds, and the corresponding carbon-carbon double bond characteristic peaks and silicon-hydrogen bond characteristic peaks appear at the same time.
[0083] According to the test, the boiling point of the radiation cross-linking sensitizer in this embodiment is 322° C., which is higher than that in Example 1. The reason is that the reaction time is prolonged and the reaction degree of TAIC with the silicone oil containing silicon-hydrogen bonds is higher.
[0084] A fluorine-containing polymer product is identical to Example 1 except that during preparation, the weight of the radiation cross-linking sensitizer is replaced by the radiation cross-linking sensitizer in this example.
[0085] Comparative Example 1:
[0086] A fluorine-containing polymer product is completely the same as Example 1 except that no radiation cross-linking sensitizer is added during the preparation.
[0087] Comparative Example 2:
[0088] A fluorine-containing polymer product is exactly the same as Example 1 except that the weight of the radiation cross-linking sensitizer is replaced by TAIC (Hunan Minhe Chemical Co., Ltd., model number FARIDA TAICS) during preparation.
[0089] Comparative Example 3:
[0090] A fluorine-containing polymer product, except that the weight of the radiation cross-linking sensitizer is replaced by TAIC and silicone oil containing silicon-hydrogen bonds (same as in Example 1; the weight ratio of TAIC to silicone oil containing silicon-hydrogen bonds is 2:1) during preparation, the rest is exactly the same as in Example 1. Performance test:
[0091] The mechanical properties test results of the fluorine-containing polymer products in Examples 1 to 7 and Comparative Examples 1 to 3 are shown in the following table:
[0092] Table 1 Mechanical properties test results of fluorinated polymer products in Examples 1 to 7 and Comparative Examples 1 to 3
[0093]
[0094] Note:
[0095] Tensile strength and elongation at break: Tested with reference to “ASTM D638 Standard Test Method for Tensile Properties of Plastics”, with a tensile speed of 50 mm / min and a test temperature of 25°C.
[0096] From Table 1, we can see that:
[0097] 1) The mechanical properties of the fluoropolymer products in Examples 1 to 7 are greatly improved compared with those in Comparative Examples 1 to 3 (the tensile strength of the fluoropolymer product in Example 4 is as high as 53.4 MPa). The reason is that the radiation cross-linking sensitizers in Examples 1 to 7 are basically not volatilized during the processing and are not easy to self-polymerize. They can be effectively mixed in the fluoropolymer and play a role in promoting cross-linking efficiently during the irradiation process. The radiation cross-linking reaction is much higher than the radiation degradation reaction, so that the fluoropolymer products can achieve ideal mechanical properties;
[0098] 2) In Comparative Example 1, the fluorine-containing polymer is directly extruded and irradiated, and there is no radiation cross-linking sensitizer to promote cross-linking during the irradiation process. The fluorine-containing polymer undergoes obvious degradation reaction during the irradiation process, which reduces the mechanical properties of the fluorine-containing polymer product;
[0099] 3) In Comparative Example 2, unmodified TAIC was added, and a large amount of TAIC self-polymerized during the processing, accompanied by volatilization, and the mechanical properties of the fluoropolymer were basically not improved after irradiation;
[0100] 4) In Comparative Example 3, TAIC and silicone oil containing silicon-hydrogen bonds were directly mixed with fluoropolymers for granulation. After processing and irradiation, the mechanical properties of the fluoropolymer products were not ideal. The reason is that there was no suitable reaction environment for TAIC and silicone oil containing silicon-hydrogen bonds to react during the processing, so it was impossible to achieve the same effect as the irradiation cross-linking sensitizer in Examples 1 to 7.
[0101] In summary, the radiation cross-linking sensitizer of the present invention has the advantages of high boiling point, good thermal stability, good cross-linking auxiliary effect, low production cost, etc. It can effectively improve the cross-linking effect of fluorine-containing polymers and reduce the degradation of molecular chains. The preparation method thereof is simple to operate and the reaction conditions are mild, and it is suitable for large-scale industrial production and application.
[0102] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A radiation cross-linking sensitizer, characterized in that: It is obtained by reacting a compound containing multiple carbon-carbon double bonds with silicone oil containing silicon-hydrogen bonds; the compound containing multiple carbon-carbon double bonds is at least one of triallyl isocyanurate, trimethallyl isocyanate and triallyl cyanurate.
2. The radiation cross-linking sensitizer according to claim 1, characterized in that: The molar ratio of the carbon-carbon double bonds in the compound containing multiple carbon-carbon double bonds to the silicon-hydrogen bonds in the silicone oil containing silicon-hydrogen bonds is 1 to 6:
1.
3. The radiation cross-linking sensitizer according to claim 1 or 2, characterized in that: The hydrogen content of the silicone oil containing silicon-hydrogen bonds is less than 2 wt %.
4. A method for preparing a radiation cross-linking sensitizer as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: A compound containing multiple carbon-carbon double bonds, an inhibitor and a catalyst are dispersed in a solvent, and then silicone oil containing silicon-hydrogen bonds is added and the temperature is raised to react, thereby obtaining a radiation cross-linking sensitizer.
5. The preparation method according to claim 4, characterized in that: The dosage of the inhibitor is 0.2% to 1.5% of the weight of the silicone oil containing silicon-hydrogen bonds; the dosage of the catalyst is 0.2% to 2% of the weight of the silicone oil containing silicon-hydrogen bonds.
6. The preparation method according to claim 4 or 5, characterized in that: The inhibitor is at least one of 1-ethynylcyclohexanol, 2-vinyl isopropanol, and 1-ethynylcyclopentanol; and the catalyst is at least one of Custer catalyst, platinum phosphate, and chloroplatinic acid.
7. The preparation method according to claim 4 or 5, characterized in that: The reaction is carried out at a temperature of 70° C. to 110° C. and the reaction time is 2 h to 10 h.
8. The preparation method according to claim 4 or 5, characterized in that: After the reaction was completed, the product was extracted with ethanol and purified by column chromatography.
9. A fluorine-containing polymer product, characterized in that The invention comprises the radiation cross-linking sensitizer according to any one of claims 1 to 3.
10. The fluorinated polymer article according to claim 9, characterized in that: The weight ratio of the fluorine-containing polymer to the radiation cross-linking sensitizer in the fluorine-containing polymer product is 100:0.05-20.
Citation Information
Patent Citations
Irradiation crosslinking sensitizer as well as preparation method and application of irradiation crosslinking sensitizer
CN104877171A
Crosslinking sensitizer for fluorine-containing polymer
CN105037797A
Sensitizer for irradiation crosslinking of fluorine-containing polymer as well as preparation method and application thereof
CN112062703A
Radiation-curable silicone rubber composition
JP2005036050A
Radiation-cross linked composition based on fluorocarbon polymer
RU2414762C1