Latent thermoplastic catalyst modified cyanate resin as well as preparation method and application thereof
By using a thermoplastic polyimide resin catalyst with a side hydroxyl structure in cyanate resin, the curing temperature is reduced, toughness and heat resistance are improved, and the shelf life is extended, solving the problem of resin performance loss caused by traditional catalysts is solved .
Patent Information
- Application Number
- CN202310555717.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
The curing temperature of existing cyanate resins is high, resulting in limited application, and traditional catalysts lose the shelf life and thermal properties of the resin when lowering the curing temperature.
Thermoplastic polyimide resin containing side hydroxyl structures is used as a catalyst. By introducing side hydroxyl groups on the main chain of the molecule, the phase separation size and aggregated structure are regulated, the curing temperature of cyanate resin is reduced, while maintaining its storage. periodic and thermal performance.
The low-temperature curing of cyanate resin is achieved, which improves its toughness and heat resistance, extends the shelf life, and maintains a high room temperature tensile strength and impact strength.
Smart Images

Figure BDA0004234099990000021 
Figure BDA0004234099990000022 
Figure BDA0004234099990000031
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer material modification, and in particular relates to a cyanate resin modified with a latent thermoplastic catalyst, a preparation method and application thereof. Background Art
[0002] Since the advent of cyanate ester resins in the 1970s and 1980s, the cyanate groups (-OCN) in their molecules undergo cyclopolymerization under the action of heat or catalysts to form a symmetrical triazine ring structure, giving cyanate ester resins excellent heat resistance, dielectric properties, mechanical properties and other properties. Compared with epoxy resins and bismaleimide resins, they have more comprehensive performance advantages and have been widely used in aviation, aerospace and electronics fields in recent years.
[0003] In general, during the cyanate curing reaction, with the formation of triazine rings, the intermolecular cross-linking density increases, the group activity weakens, and the degree of curing reaction is limited. It is usually necessary to cure at 230°C or above to increase the degree of curing in order to achieve ideal comprehensive performance. This is limited in some application scenarios. For example, in foam sandwich antenna cover materials, the temperature resistance of the foam sandwich material generally does not exceed 180°C, and it is impossible to achieve co-curing molding with cyanate resins with a curing temperature of 230°C or above. In addition, during the cooling process of cyanate resin composites cured at 230°C or above to room temperature, residual stress is easily generated inside the material due to the inconsistent thermal expansion coefficients of the resin and fiber in the composite material, which makes the product easy to deform during use and affects the interlayer performance of the composite material. Therefore, lowering the curing temperature of cyanate resin and expanding its application field is one of the important research directions.
[0004] To lower the curing reaction temperature of cyanate ester resins and increase the degree of reaction, most catalysts currently use transition metal complexes such as acetylacetonate and organotin as primary catalysts, with active hydrogen compounds such as nonylphenol and other small molecule compounds as auxiliary catalysts. Transition metal complexes can significantly lower the resin curing temperature, but this also reduces the resin's shelf life at room temperature. Small molecule compounds containing active hydrogen, such as nonylphenol, have a weak catalytic effect when added in small amounts, while large additions can lead to significant thermal performance losses in the resin system. Therefore, catalysts are generally required to have a long shelf life at room temperature to ensure stable processability of the resin, and a long processing window between room temperature and gel temperature, such as for the stable preparation of prepregs for resin-based composites and the control of the pressure point in autoclave processes.
[0005] After curing, traditional cyanate ester resins form a dense triazine ring structure. Although their mechanical properties are superior to those of AG-80 / DDS epoxy resin systems and BMI / DABPA bismaleimide resin systems, they still cannot meet the toughness requirements of advanced resin-based composites. For example, winding-molded engine casings require a resin elongation at break of 3.2 or above and a tensile strength of 80 MPa or above. Currently, the most successful methods for modifying cyanate ester resins are thermoplastic resins such as polycarbonate (PC), polysulfone (PSF), polyetherketone (PEK), polyetheretherketone (PEEK), polyethersulfone (PES), and polyetherimide (PEI). These methods can also minimize the loss of thermal performance of cyanate ester resins. Patents such as US5527592A, US5143785A, and CN102127224B describe the performance of thermoplastic resin-modified cyanate ester resins. The thermoplastic resins used contain almost no reactive functional groups or have a very low concentration of reactive functional groups.
[0006] Therefore, there is an urgent need to develop a new resin system that can significantly reduce the curing temperature of the cyanate ester resin system while maintaining a relatively high room temperature shelf life while also having excellent toughness and heat resistance. The present invention avoids the technical problems of short shelf life, poor mechanical properties, and low heat resistance caused by small molecule catalysts in modified cyanate ester resins, and has very important application value. Summary of the Invention
[0007] The present invention provides a cyanate ester resin modified with a latent thermoplastic catalyst, a preparation method and an application thereof. The modified cyanate ester resin of the present invention has a low curing temperature, a long room temperature storage period, excellent mechanical properties and high heat resistance.
[0008] The present invention provides a latent thermoplastic catalyst-modified cyanate resin, which is prepared from the following raw materials in parts by weight:
[0009] Cyanate resin: 100 parts, thermoplastic catalyst: 15-40 parts, reactive diluent: 5-15 parts;
[0010] The thermoplastic catalyst is a thermoplastic polyimide resin containing a side hydroxyl structure in the main chain of the molecule, having a structure shown in Formula I.
[0011]
[0012] In formula I, m and n are the numbers of structural units, respectively, m is an integer ≥20, and n is an integer ≥0; 20≤m+n≤100, R1 is an aromatic dianhydride monomer, R2 is an aromatic diamine monomer containing a hydroxyl structure, and R3 is an aromatic diamine monomer not containing a hydroxyl structure.
[0013] Preferably, R1 is one or more of Formulas 1-1 to 1-11:
[0014]
[0015] Preferably, R2 is one or more of Formula 2-1 to Formula 2-6:
[0016]
[0017] Preferably, R3 is one or more of Formula 3-1 to Formula 3-26:
[0018]
[0019] Preferably, the thermoplastic catalyst has an inherent viscosity of 0.25 to 1.5 dL / g, a glass transition temperature of 230 to 300° C., an elongation at break of ≥20%, and a mesh size of 300 to 1000 meshes.
[0020] The present invention provides a method for preparing the above-mentioned latent thermoplastic catalyst-modified cyanate ester resin, comprising the following steps:
[0021] A) stirring a cyanate resin and a portion of a thermoplastic catalyst under heating conditions to perform a prepolymerization reaction to obtain a prepolymerized intermediate resin M1;
[0022] B) stirring and mixing the prepolymerized intermediate resin with a reactive diluent, and reacting until no crystals are precipitated at room temperature, to obtain an intermediate resin M2;
[0023] C) Mechanically mixing the remaining thermoplastic catalyst with the intermediate resin M2 and reacting them to obtain a latent thermoplastic catalyst-modified cyanate ester resin.
[0024] Preferably, the mass of the part of the thermoplastic catalyst in step A) accounts for 15 to 50% of the total mass of the thermoplastic catalyst;
[0025] In the step A), the cyanate resin and part of the thermoplastic catalyst are stirred at a speed of 200 to 2000 r / min and kept at a constant temperature of 110 to 170° C. for 1 to 10 hours.
[0026] Preferably, the reaction temperature in step B) is 90-150° C., and the reaction time is 1-8 hours;
[0027] In step B), the stirring speed is 100 to 1500 r / min;
[0028] The reaction temperature in step C) is 50-100° C., and the reaction time is 30-60 minutes.
[0029] The present invention provides the application of the above-mentioned latent thermoplastic catalyst-modified cyanate ester resin in the fields of aviation, aerospace and electronics.
[0030] Preferably, the latent thermoplastic catalyst-modified cyanate ester resin is cured to obtain a modified cyanate ester resin cured product, which is used in the fields of aviation, aerospace and electronics;
[0031] The glass transition temperature of the modified cyanate ester resin cured product is ≥250°C, the tensile strength of the modified cyanate ester at room temperature is ≥85MPa, the elongation at break is ≥3.5%, and the impact strength is ≥25kJ / m 2 Compared with the tensile strength of the resin at room temperature, the tensile strength retention rate of the resin at 177°C is ≥50%, and the thermal decomposition temperature of 5% is ≥410°C.
[0032] The invention provides a cyanate ester resin modified with a latent thermoplastic catalyst. The cyanate ester resin is prepared from the following raw materials in parts by weight: 100 parts of a cyanate ester resin, 15 to 40 parts of a thermoplastic catalyst, and 5 to 15 parts of a reactive diluent. The thermoplastic catalyst is a thermoplastic polyimide resin containing a side hydroxyl structure in a molecular main chain and has a structure shown in Formula I. In Formula I, m and n are respectively the number of structural units, m is an integer ≥20, and n is an integer ≥0; 20≤m+n≤100, R1 is an aromatic dianhydride monomer, R2 is an aromatic diamine monomer containing a hydroxyl structure, and R3 is an aromatic diamine monomer not containing a hydroxyl structure.
[0033] The latent thermoplastic catalyst-modified cyanate resin of the present invention and its preparation method have the following advantages:
[0034] (1) A macromolecular thermoplastic polyimide resin containing side active hydroxyl groups on the main chain is used as a thermoplastic catalyst. The side hydroxyl groups on the main chain can quickly promote the cross-linking and curing of the cyanate resin as the temperature rises. The glass transition temperature of the cyanate resin after curing at 180±5℃ reaches 250℃ or above.
[0035] (2) The thermoplastic catalyst main chain is composed of a high-temperature resistant and high-toughness polyimide resin with an imide ring and / or an oxygen ether bond bridge, with a glass transition temperature of 230-300°C and an elongation at break of ≥20%. The side hydroxyl groups can regulate the phase separation size and aggregation structure during the curing process of the cyanate ester resin, so that the prepared modified cyanate ester resin has both high toughness and high temperature resistance. The tensile strength of the modified cyanate ester at room temperature is ≥85MPa, and the impact strength is ≥25KJ / m 2 , compared with the tensile strength of the resin at room temperature, the tensile strength retention rate of the resin at 177°C is ≥50%.
[0036] (3) The thermoplastic catalyst is a thermoplastic polyimide resin containing side active hydroxyl groups on the main chain. On the one hand, the molecular weight is between 10,000 and 100,000, and the active hydroxyl groups on the side of the main chain have low activity at room temperature. On the other hand, the active hydroxyl groups in the molecular structure of the thermoplastic catalyst form hydrogen bonds with the carbonyl groups on the adjacent amide rings to form a seven-membered ring, as shown in Figures 2 and 3. This reduces the activity of the hydroxyl groups at room temperature, and can maintain a long storage period of the modified cyanate ester resin system at room temperature, which can reach more than 60 days. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0038] Figure 1 Schematic diagram of the curing process of the cyanate ester modified with a latent thermoplastic catalyst of the present invention;
[0039] Figure 2 This is a DSC graph of the cyanate modified with a latent thermoplastic catalyst according to Example 1 of the present invention;
[0040] Figure 3 This is a temperature-dependent rheological diagram of a cyanate modified with a latent thermoplastic catalyst according to Example 1 of the present invention;
[0041] Figure 4 The constant temperature rheological diagram of the cyanate modified with a latent thermoplastic catalyst prepared in Example 3 of the present invention;
[0042] Figure 5 This is the DMA graph of the thermoplastic polyimide-modified cyanate ester cured product of Comparative Example 1 of the present invention;
[0043] Figure 6 This is a DMA graph of a cyanate cured product modified with a latent thermoplastic catalyst according to Example 1 of the present invention;
[0044] Figure 7 This is a TGA graph of a cyanate cured product modified with a latent thermoplastic catalyst according to Example 5 of the present invention. DETAILED DESCRIPTION
[0045] The present invention provides a latent thermoplastic catalyst-modified cyanate resin, which is prepared from the following raw materials in parts by weight:
[0046] Cyanate resin: 100 parts, thermoplastic catalyst: 15-40 parts, reactive diluent: 5-15 parts;
[0047] In the present invention, the cyanate resin preferably includes one or more of 4,4'-dicyanate diphenylpropane, 4,4'-dicyanate diphenylmethane, 4,4'-dicyanate diphenylbutane, 4,4'-methylenebis(2,6-dimethylphenylcyanate), 2,2-bis(4-cyanate-3,5-dimethylphenyl)propane, 4,4'-[1,3-phenylbis(1-methyl-ethylene)]bisphenylcyanate, 4,4'-dicyanate diphenylhexafluoropropane, 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-dicyanate, 4,4'-dicyanate diphenyl sulfone, dicyclopentadiene type cyanate and phenolic type cyanate.
[0048] In the present invention, the thermoplastic catalyst is a thermoplastic polyimide resin containing a side hydroxyl structure in the main chain of the molecule, having a structure shown in Formula I,
[0049]
[0050] In formula I, m and n are the number of structural units, respectively, m is an integer ≥20, and n is an integer ≥0; 20≤m+n≤100, R1 is an aromatic dianhydride monomer, R2 is an aromatic diamine monomer, and R3 is an aromatic diamine monomer.
[0051] In the present invention, the weight fraction of the thermoplastic catalyst is preferably 15 to 40 parts, more preferably 20 to 35 parts, such as 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, preferably a range with any of the above values as the upper or lower limit.
[0052] In the present invention, the thermoplastic catalyst is a thermoplastic polyimide resin containing a side hydroxyl structure in the main chain of the molecule, having a structure shown in Formula I. It has strong catalytic performance on cyanate esters and simultaneously has both mechanical properties and heat resistance of thermoplastic polyimide resins. First, by designing the molecular structure, the active side hydroxyl group is introduced into the molecular structure. By regulating the molecular structure and molecular weight, the resin can be dissolved in conventional low-boiling organic solvents and melted in the cyanate resin system. The cross-linking and curing of the cyanate resin is catalyzed by the side hydroxyl active groups in the thermoplastic catalyst polymer. During the co-curing process, the phase separation size and the aggregate structure can be better regulated, thereby achieving a high toughening effect on the cyanate resin. Secondly, the designed thermoplastic catalyst has high heat resistance, a glass transition temperature of 230 to 300°C, and excellent high-temperature mechanical properties. When it is introduced into the cyanate resin system, the heat resistance of the resin system is almost not lost. The final designed catalyst is a macromolecule with a number-average molecular weight between 10,000 and 100,000, and the active hydroxyl group in the molecular structure forms an intramolecular hydrogen bond with the carbonyl group on the adjacent amide ring to form a seven-membered ring. This makes the thermoplastic catalyst low in activity at room temperature, and adding it to the cyanate ester resin system can maintain a longer storage period of the cyanate ester resin system.
[0053] In Formula I, m and n are the number of structural units, respectively, m is an integer ≥20, preferably, 20≤m≤100, more preferably, 30≤m≤80, such as m is 20, 30, 40, 50, 60, 70, 80, 90, 100; n is an integer ≥0, preferably, 0≤n≤100, more preferably, 10≤n≤80, such as 0, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100; 20≤m+n≤100, preferably, 30≤m+n≤90, more preferably, 40≤m+n≤80.
[0054] In the present invention, R1 is one or more of Formulas 1-1 to 1-11:
[0055]
[0056] R2 is one or more of Formula 2-1 to Formula 2-6:
[0057]
[0058] R3 is one or more of Formula 3-1 to Formula 3-26:
[0059]
[0060] In the structural formula of the present invention, "—" represents a connecting bond, and "—*" represents a connecting bond between R2 and the hydroxyl group.
[0061] In the present invention, the thermoplastic catalyst has an inherent viscosity of 0.25 to 1.5 dL / g, a glass transition temperature of 230 to 300° C., an elongation at break of ≥20%, and a mesh size of 300 to 1000 meshes.
[0062] The thermoplastic catalyst of the present invention can be prepared by a conventional one-step or two-step method for preparing polyimide resin, which is a technical content well known to those skilled in the art. The present invention preferably prepares the thermoplastic catalyst having the structure shown in Formula I by the following two-step method:
[0063] (1) dissolving a diamine monomer, a dianhydride monomer, and phthalic anhydride in an organic solvent and stirring the mixture for 10 to 12 hours at 4 to 10° C. to obtain a polyimide acid intermediate. In this process, the organic solvent is preferably N,N-dimethylacetamide;
[0064] (2) Add the intermediate product obtained in step (1) to a water-containing solvent, raise the temperature to 150-180°C, continue stirring and reacting for 8-10 hours, and at the same time, separate the distilled xylene and water mixture in a water separator, and the water removal is completed. After cooling to room temperature, the solution is slowly poured into anhydrous ethanol for precipitation, and the precipitate is placed in a Soxhlet extractor and subjected to a heating cycle treatment with anhydrous ethanol for 2 days. After vacuum drying at 185-215°C for 2-4 hours, 235-265°C for 2-4 hours, and 300°C for 1-2 hours, the thermoplastic catalyst (Formula 1) of the present invention is obtained. The water-containing solvent is preferably xylene.
[0065] In the present invention, the diamine monomer includes a diamine monomer containing a hydroxyl structure and a diamine monomer not containing a hydroxyl structure. The diamine monomer containing a hydroxyl structure preferably includes one or more of 4,6-diaminoresorcinol, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 3,3'-dihydroxybenzidine (P-HAB), 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAP), 2-amino-4-[(3-amino-4-hydroxyphenyl)methyl]phenol, and 3,3'-diamino-4,4'-biphenylglycol.
[0066] The diamine monomers not containing a hydroxyl structure preferably include 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine (TFMB); 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether (6FODA), 9,9-(3-fluoro-4-aminophenyl)fluorene (FFDA), 3,4'-diaminodiphenyl ether (3,4'-ODA), 4,4'-diaminodiphenyl ether (4,4'-ODA), 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3, 3,3-Hexafluoropropane (HFBAPP), 2,2-bis[4-(4-aminophenoxy)phenyl]-propane (BAPP), 4,4'-diamino-2,2'-dimethylbiphenyl (M-Tolidine), 4,4'-bis(3-aminophenoxy)diphenyl sulfone (BAPS-M), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 2-(4-aminophenoxy)-5-aminobiphenyl (P-ODA), 1,3-bis(4'-aminophenoxy)benzene (TPE-R), 1,3-bis(4'-aminophenoxy)benzene (3-Aminophenoxy)benzene (APB), 4,4'-bis(4-aminophenoxy)biphenyl (BAPB), 1,4-bis(4-aminophenoxy)-2-phenylbenzene (P-APB), 3,3'-dimethylbenzidine (O-Tolidine), 3,3',5,5'-tetramethylbenzidine (TMB), m-phenylenediamine (MPD), 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane oropropane), 2,2-bis(4-aminophenyl)hexafluoropropane, 2,4-diaminotoluene, 4,4-diaminobiphenyl-2,2'-dicarboxylic acid, 9,9-dimethylfluorene-2,7-diamine, 4,4-diaminodiphenylmethane, 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene, 5(6)-1-(4-aminophenyl)-1,3,3-trimethylindane.
[0067] In the present invention, the dianhydride monomer preferably includes one or more of 2,3,3',4'-biphenyltetracarboxylic dianhydride (α-BPDA), 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride (α-ODPA), hexafluorodianhydride (6FDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), bisphenol A diether dianhydride (BPADA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (BPAF), 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride (DSDA), 3,3',4,4'-biphenyl ether dianhydride (ODPA), 4,4'-terephthalic anhydride (HQDPA), and (4-phthalic anhydride) formyloxy-4-phthalate (8CI).
[0068] In the present invention, the amounts of the diamine monomer, dianhydride monomer and phthalic anhydride can be adjusted according to the structure shown in Formula I, which is a technical means well known to those skilled in the art and will not be described in detail herein.
[0069] The active hydroxyl group in the molecular structure of the thermoplastic catalyst of the present invention forms a hydrogen bond with the carbonyl group on the adjacent amide ring to form a seven-membered ring, as shown in Formula II.
[0070]
[0071] For example, when R1 is hexafluorodianhydride (6FDA), R2 is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), and R3 is 4,4'-diaminodiphenyl ether (4,4'-ODA), the structure of the thermoplastic catalyst is as shown in Formula III.
[0072]
[0073] In the present invention, the reactive diluent is preferably one or more of 4,4'-dicyanate diphenylethane, phenol cyanate, tert-butylphenol cyanate, 4-cumylphenol cyanate, styrenephenol cyanate and nonylphenol cyanate; the weight fraction of the reactive diluent is preferably 5 to 15 parts, more preferably 8 to 12 parts, such as 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, preferably a range value with any of the above values as the upper or lower limit.
[0074] The present invention also provides a method for preparing the above-mentioned latent thermoplastic catalyst-modified cyanate ester resin, comprising the following steps:
[0075] A) stirring a cyanate resin and a portion of a thermoplastic catalyst under heating conditions to obtain a prepolymerized intermediate resin M1;
[0076] B) stirring and mixing the prepolymerized intermediate resin with a reactive diluent, and reacting until no crystals are precipitated at room temperature, to obtain an intermediate resin M2;
[0077] C) Mechanically mixing the remaining thermoplastic catalyst with the intermediate resin M2 and reacting them to obtain a latent thermoplastic catalyst-modified cyanate ester resin.
[0078] In the present invention, the types and amounts of the cyanate resin, thermoplastic catalyst and reactive diluent are consistent with those described above, and are not further described herein.
[0079] In the present invention, the mass of the part of the thermoplastic catalyst added first accounts for 15-50% of the total mass of the thermoplastic catalyst, more preferably 20-45%, such as 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, preferably a range with any of the above values as the upper or lower limit.
[0080] In the present invention, the reaction of the cyanate ester resin and part of the thermoplastic catalyst is carried out under stirring. The stirring speed is preferably 200-2000 r / min, more preferably 500-1500 r / min, such as 200 r / min, 500 r / min, 800 r / min, 1000 r / min, 1200 r / min, 1500 r / min, 1800 r / min, 2000 r / min, and preferably a range value with the above arbitrary numerical values as the upper or lower limit; the temperature of the prepolymerization reaction is preferably 110-170°C, more preferably 120-150°C, such as 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, and preferably a range value with the above arbitrary numerical values as the upper or lower limit; the constant temperature holding time at the above temperature is preferably 1-10 hours, more preferably 3-8 hours, and most preferably 5-6 hours.
[0081] After obtaining the intermediate resin M1, the present invention cools the prepolymerized intermediate resin M1 to 90-150° C., adds a reactive diluent under stirring at a speed of 100 r / min-1500 r / min, and continues to keep the temperature for 1-8 hours until no crystals are precipitated from the resin at room temperature to obtain the intermediate resin M2;
[0082] In the present invention, the intermediate resin M1 is preferably cooled to 90-150°C, more preferably 100-130°C, such as 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, preferably with any of the above values as the upper or lower limit; after adding the reactive diluent, it is preferably kept at the above temperature for 1-8 hours, more preferably 3-6 hours, and most preferably 4-5 hours. The above reaction is preferably carried out under stirring conditions, and the stirring speed is preferably 100-1500r / min, more preferably 300-1200r / min, such as 100r / min, 300r / min, 500r / min, 800r / min, 1000r / min, 1200r / min, 1500r / min, preferably with any of the above values as the upper or lower limit.
[0083] The prepared intermediate resin M2 is then added to a mechanical mixing device and heated to 50-100°C. The remaining thermoplastic catalyst is added to M2 and dispersed for 30-60 minutes to obtain a uniform resin, which is the modified cyanate ester resin. In the present invention, the mechanical mixing device preferably includes one or more of a high-speed disperser, a grinder, and an internal mixer.
[0084] In the present invention, the prepared M2 is preferably heated to 50-100°C, more preferably 60-80°C, such as 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, preferably with any of the above values as the upper or lower limit of the range value; the dispersion time is preferably 30-60min, more preferably 40-50min.
[0085] The present invention also provides a method for preparing a cured product of a latent thermoplastic catalyst modified cyanate ester resin, which comprises curing the aforementioned latent thermoplastic catalyst and its modified cyanate ester resin to obtain a cured product of the latent thermoplastic catalyst and its modified cyanate ester resin.
[0086] The specific curing process is as follows:
[0087] The latent thermoplastic catalyst modified cyanate resin described above is heated to 80-130° C., degassed at a vacuum pressure of -0.1-0 MPa for 30-60 min, and then cured according to a heating program of keeping at 115-135° C. for 1-3 h, keeping at 145-160° C. for 2-4 h, and keeping at 175-185° C. for 4-6 h to obtain a modified cyanate resin cured product.
[0088] The present invention also provides the use of the above-mentioned latent thermoplastic catalyst modified cyanate ester resin or the latent thermoplastic catalyst modified cyanate ester resin cured product in the fields of advanced aerospace resin-based composite materials, adhesives, and electronic information.
[0089] The invention provides a latent thermoplastic catalyst modified cyanate ester resin having low melt viscosity and good solvent solubility, which can realize melt impregnation and solution impregnation of the reinforcing material in the above applications.
[0090] The invention provides a cyanate ester resin modified with a latent thermoplastic catalyst. The cyanate ester resin is prepared from the following raw materials in parts by weight: 100 parts of a cyanate ester resin, 15 to 40 parts of a thermoplastic catalyst, and 5 to 15 parts of a reactive diluent. The thermoplastic catalyst is a thermoplastic polyimide resin containing a side hydroxyl structure in a molecular main chain and has a structure shown in Formula I. In Formula I, m and n are respectively the number of structural units, m is an integer ≥20, and n is an integer ≥0; 20≤m+n≤100, R1 is an aromatic dianhydride monomer, R2 is an aromatic diamine monomer containing a hydroxyl structure, and R3 is an aromatic diamine monomer not containing a hydroxyl structure.
[0091] The latent thermoplastic catalyst-modified cyanate resin of the present invention and its preparation method have the following advantages:
[0092] (1) A macromolecular thermoplastic polyimide resin containing side active hydroxyl groups on the main chain is used as a thermoplastic catalyst. The side hydroxyl groups on the main chain can quickly promote the cross-linking and curing of the cyanate resin as the temperature rises. The glass transition temperature of the cyanate resin after curing at 180±5℃ reaches 250℃ or above.
[0093] (2) The thermoplastic catalyst main chain is composed of a high-temperature resistant and high-toughness polyimide resin with an imide ring and / or an oxygen ether bond bridge, with a glass transition temperature of 230-300°C and an elongation at break of ≥20%. The side hydroxyl groups can regulate the phase separation size and aggregation structure during the curing process of the cyanate ester resin, so that the prepared modified cyanate ester resin has both high toughness and high temperature resistance. The tensile strength of the modified cyanate ester at room temperature is ≥85MPa, and the impact strength is ≥25KJ / m 2 , compared with the tensile strength of the resin at room temperature, the tensile strength retention rate of the resin at 177°C is ≥50%.
[0094] (3) The thermoplastic catalyst is a thermoplastic polyimide resin containing side active hydroxyl groups on the main chain. On the one hand, the molecular weight is between 10,000 and 100,000, and the active hydroxyl groups on the side of the main chain have low activity at room temperature. On the other hand, the active hydroxyl groups in the molecular structure of the thermoplastic catalyst form hydrogen bonds with the carbonyl groups on the adjacent amide rings to form a seven-membered ring, as shown in Figures 2 and 3. This reduces the activity of the hydroxyl groups at room temperature, and can maintain a long storage period of the modified cyanate ester resin system at room temperature, which can reach more than 60 days.
[0095] To further illustrate the present invention, a latent thermoplastic catalyst-modified cyanate ester resin provided by the present invention, its preparation method and application are described in detail below with reference to the examples, but they should not be construed as limiting the scope of protection of the present invention.
[0096] In the following comparative examples and examples, the intrinsic viscosity test conditions of the thermoplastic polyimide resin and the latent thermoplastic catalyst are as follows: 0.125 g of sample is prepared into 25 ml of N-methylpyrrolidone solution and tested using an Ubbelohde viscometer at 30°C;
[0097] In the following comparative examples and examples, the glass transition temperature test conditions of the thermoplastic polyimide resin and the latent thermoplastic catalyst are as follows: DMA test, film stretching mode, frequency 1 Hz, heating rate 5 ° C / min;
[0098] In the following comparative examples and examples, the elongation at break of thermoplastic polyimide resin and latent thermoplastic catalyst was tested in accordance with GB / T1040.3-2006.
[0099] In the following comparative examples and examples, the solubility test conditions for the thermoplastic polyimide resin, the latent thermoplastic catalyst, and the modified cyanate ester resin were as follows: the resin and solvent were weighed at a concentration of 10 mg / ml. If the resin was completely dissolved at room temperature, it was marked as "++". If the resin was completely dissolved under heating, it was marked as "+".
[0100] In the following comparative examples and examples, the gel time test conditions of the modified cyanate ester resin at 150°C are as follows: the test is carried out according to the national military standard GJB1059.4;
[0101] In the following comparative examples and examples, the room temperature storage period test conditions of the modified cyanate ester resin are: the test temperature is 23±2°C, and the time required for the viscosity of the test resin to double at this temperature;
[0102] In the following comparative examples and examples, the rheological test conditions for the modified cyanate ester resin are as follows: 1. Constant temperature viscosity change test, using a high-temperature extensional rheometer in oscillation mode, at 80°C, a hold time of 4 hours, a strain of 1.0%, an angular frequency of 10.0 rad / s, and an air atmosphere. 2. Varying temperature viscosity change test, using a high-temperature extensional rheometer in oscillation mode, at a test temperature of 60-200°C, with a heating rate of 1°C / min.
[0103] In the following comparative examples and examples, the DSC test conditions for the modified cyanate ester resin are as follows: temperature range: 40-350°C, heating rate: 5°C / min;
[0104] In the following comparative examples and examples, the test conditions for the glass transition temperature of the modified cyanate ester resin cured product are: DMA test, single cantilever beam mode, frequency 1 Hz, heating rate 5 ° C / min;
[0105] In the following comparative examples and examples, the test conditions for the 5% thermal weight loss temperature of the modified cyanate ester resin cured product are: a heating rate of 10°C / min, a temperature range of 40 to 800°C, and a nitrogen atmosphere;
[0106] In the following comparative examples and examples, the tensile properties, flexural properties and impact strength of the modified cyanate ester resin cured products were tested according to the national standard GB / T2567-2008.
[0107] Example 1
[0108] The method for preparing a thermoplastic catalyst comprises the following steps:
[0109] Under nitrogen, 0.1 mol of diamine monomer (containing 0.07 mol of 4,6-diaminoresorcinol and 0.03 mol of 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor. The mixture was stirred at room temperature. After the diamine monomer was completely dissolved, 0.05 mol of 2,3,3',4'-biphenyltetracarboxylic dianhydride and 0.05125 mol of 3,3',4,4'-biphenyl ether dianhydride were added. Stirring was continued at 5°C for 12 hours to prepare the intermediate polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 160°C. Stirring was continued for 10 hours. A mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was heated under reflux in the ethanol in a Soxhlet extractor for two days and then vacuum-dried at 190°C for 3 hours, 245°C for 4 hours, and 300°C for 2 hours to obtain a pale yellow thermoplastic catalyst, designated C-1. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.48 dL / g, a glass transition temperature of 288°C, and an elongation at break of 48%. The catalyst was crushed to a 400-mesh size.
[0110] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated by weight: 100 parts of 4,4'-dicyanate diphenyl propane, 20 parts of thermoplastic catalyst (C-1), and 10 parts of 4-cumylphenol cyanate;
[0111] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0112] (1) Weigh the raw materials according to the required proportions by weight;
[0113] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of the thermoplastic catalyst weighed in step (1) at 140° C. under stirring conditions at a speed of 800 r / min for 5 h, until the component resins are uniformly melted to obtain a pre-polymerized intermediate resin M1;
[0114] (3) Cooling the prepolymerized intermediate resin M1 to 110° C., adding 10 parts of the active diluent 4-cumylphenol cyanate weighed in step (1) under stirring at a speed of 200 r / min, and continuing to keep warm for 2 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0115] (4) The intermediate resin M2 prepared in step (3) is added to a high-speed disperser and heated to 90° C. The remaining 10 parts of the thermoplastic catalyst in step 1 are added to M2 and dispersed for 45 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0116] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0117] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.09 MPa for 40 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130° C. / 2 h+150° C. / 3 h+180° C. / 5 h to obtain a cured thermoplastic catalyst-modified cyanate ester resin.
[0118] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0119] Example 2
[0120] The method for preparing a thermoplastic catalyst comprises the following steps:
[0121] Under nitrogen, 0.1 mol of diamine monomer (comprising 0.06 mol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 0.04 mol of 3,4'-diaminodiphenyl ether, and 500 ml of N,N'-dimethylacetamide) was added to a 1000 ml reactor. The mixture was stirred at room temperature. After the diamine monomer was completely dissolved, 0.04 mol of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride and 0.0625 mol of hexafluorodianhydride were added. Stirring was continued at 5°C for 12 hours to prepare the intermediate polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 170°C. Stirring was continued for 10 hours. A mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was heated under reflux in the ethanol in a Soxhlet extractor for two days and then vacuum-dried at 210°C for 4 hours, 255°C for 3 hours, and 300°C for 1 hour to obtain a pale yellow thermoplastic catalyst, designated C-2. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.42 dL / g, a glass transition temperature of 295°C, and an elongation at break of 39%. The catalyst was crushed to a 500-mesh size.
[0122] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated by weight: 60 parts of 4,4'-dicyanatodiphenylpropane, 40 parts of 4,4'-methylenebis(2,6-dimethylphenylcyanate), 15 parts of thermoplastic catalyst (C-2), and 8 parts of tert-butylphenol cyanate;
[0123] The preparation method of the latent thermoplastic catalyst modified cyanate ester is the same as that of Example 1;
[0124] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0125] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 130° C., and degassed under a vacuum pressure of -0.09 MPa for 40 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130° C. / 4 h+155° C. / 2 h+185° C. / 4 h to obtain a thermoplastic catalyst-modified cyanate ester resin cured product.
[0126] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0127] Example 3
[0128] The method for preparing a thermoplastic catalyst comprises the following steps:
[0129] Under nitrogen, 0.1 mol of diamine monomer (containing 0.08 mol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 0.02 mol of 4,4'-diaminodiphenyl ether) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor. The mixture was stirred at room temperature. After the diamine monomer was completely dissolved, 0.03 mol of 2,3,3',4'-biphenyltetracarboxylic dianhydride, 0.05 mol of hexafluorodianhydride, and 0.0225 mol of 3,3',4,4'-benzophenonetetracarboxylic dianhydride were added. Stirring was continued at 4°C for 12 hours to prepare the intermediate polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 175°C. Stirring was continued for 10 hours. A mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was then heated under reflux in the ethanol in a Soxhlet extractor for two days. The catalyst was then vacuum-dried at 205°C for 4 hours, 240°C for 2-4 hours, and 300°C for 1 hour to obtain a pale yellow thermoplastic catalyst, designated C-3. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.38 dL / g, a glass transition temperature of 282°C, and an elongation at break of 27%. The catalyst had a mesh size of 325 after crushing using a pulverizer.
[0130] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated by weight: 100 parts of 4,4'-dicyanate diphenyl propane, 25 parts of thermoplastic catalyst (C-3), and 10 parts of 4-cumylphenol cyanate;
[0131] The preparation method of the latent thermoplastic catalyst modified cyanate ester is the same as that of Example 1;
[0132] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0133] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.09 MPa for 50 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 125° C. / 5 h+150° C. / 3 h+180° C. / 6 h to obtain a cured thermoplastic catalyst-modified cyanate ester resin.
[0134] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0135] Example 4
[0136] The method for preparing a thermoplastic catalyst comprises the following steps:
[0137] Under nitrogen protection, 0.1 mol of diamine monomer (which contains 0.05 mol of 3,3'-dihydroxybenzidine, 0.03 mol of 4,4'-bis(3-aminophenoxy)diphenyl sulfone, 0.02 4,4'-diamino-2,2'-dimethylbiphenyl and 500 ml of N,N'-dimethylacetamide) was added to a 1000 ml reactor and stirred at room temperature. After the diamine monomer was completely dissolved, 0.03 mol of bisphenol A type diether dianhydride, 0.031 mol of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride and 0.04 mol of 3,3',4,4'-biphenyltetracarboxylic dianhydride were added and stirred at 6 ° C for 12 hours to prepare an intermediate product polyimide acid solution. 200 ml of xylene was added to the solution, the temperature was raised to 155 ° C and the reaction was continued with stirring for 10 hours. At the same time, the reaction mixture was separated. A water separator separated the distilled xylene and water mixture, yielding a thermoplastic catalyst solution containing pendant hydroxyl groups. The resin solution was added to 2000 ml of ethanol to yield a thermoplastic catalyst precipitate. The precipitate was heated under reflux in ethanol in a Soxhlet extractor for two days and then vacuum-dried at 205°C for 3 hours, 255°C for 4 hours, and 300°C for 2 hours to yield a pale yellow thermoplastic catalyst, designated C-4. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.58 dL / g, a glass transition temperature of 247°C, and an elongation at break of 54%. The precipitate had a mesh size of 1000 after pulverization in a pulverizer.
[0138] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated in parts by weight: 30 parts of 4,4'-dicyanate diphenylmethane, 20 parts of 4,4'-[1,3-phenylbis(1-methyl-ethylene)]bisphenylcyanate, 50 parts of 4,4'-dicyanate diphenyl sulfone, 10 parts of thermoplastic catalyst (C-1, 15 parts of C-4), and 15 parts of 4,4'-dicyanate diphenylethane;
[0139] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0140] (1) Weigh the raw materials according to the required proportions by weight;
[0141] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of the thermoplastic catalyst (C-1) weighed in step (1) at 150° C. for 3 h under stirring conditions at a speed of 1000 r / min until the component resins are uniformly melted to obtain a prepolymerized intermediate resin M1;
[0142] (3) Cooling the prepolymerized intermediate resin M1 to 120° C., adding 10 parts of the active diluent 4-cumylphenol cyanate weighed in step (1) under stirring at a speed of 400 r / min, and continuing to keep warm for 4 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0143] (4) The intermediate resin M2 prepared in step (3) was added to an internal mixer and heated to 80°C. The remaining thermoplastic catalyst (15 parts of C-4) in step 1 was added to M2 and dispersed for 50 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0144] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0145] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 125° C., and degassed under a vacuum pressure of -0.09 MPa for 35 minutes. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130° C. / 3 h+145° C. / 4 h+175° C. / 6 h to obtain a cured thermoplastic catalyst-modified cyanate ester resin.
[0146] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0147] Example 5
[0148] The method for preparing a thermoplastic catalyst comprises the following steps:
[0149] Under nitrogen protection, 0.1 mol of diamine monomer (including 0.06 mol of 2,2-bis(3-amino-4-hydroxyphenyl)propane, 0.02 mol of 1,4-bis(4-aminophenoxy)benzene, 0.02 mol of 2,2-bis[4-(4-aminophenoxy)phenyl]-propane) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor and stirred at room temperature. After the diamine monomer was completely dissolved, 0.04 mol of 2,3,3',4'-biphenyltetracarboxylic dianhydride, 0.03 mol of 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride and 0.0305 mol of 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride were added, and stirring was continued at 5 ° C for 12 hours to prepare an intermediate product polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 170°C, with stirring and reaction continued for 8 hours. Simultaneously, a mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was heated in ethanol and refluxed in a Soxhlet extractor for 2 days. The precipitate was then vacuum-dried at 205°C for 2 hours, 250°C for 4 hours, and 300°C for 2 hours to obtain a pale yellow thermoplastic catalyst, designated C-5. The intrinsic viscosity was 0.79 dL / g, the glass transition temperature was 298°C, and the elongation at break was 34% as measured by an Ubbelohde viscometer. After pulverization in a crusher, the mesh size was 800.
[0150] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated in parts by weight: 40 parts of 4,4'-dicyanate diphenyl propane, 20 parts of 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-dicyanate, 40 parts of 2,2-bis(4-cyanate-3,5-dimethylphenyl) propane, thermoplastic catalysts (10 parts of C-2, 10 parts of C-3, 10 parts of C-5), and 10 parts of nonylphenol cyanate;
[0151] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0152] (1) Weigh the raw materials according to the required proportions by weight;
[0153] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of the thermoplastic catalyst (C-3) weighed in step (1) at 155° C. for 3 h under stirring conditions at a speed of 1000 r / min until the component resins are uniformly melted to obtain a prepolymerized intermediate resin M1;
[0154] (3) Cooling the prepolymerized intermediate resin M1 to 110° C., adding 10 parts of the active diluent nonylphenol cyanate weighed in step (1) under stirring at a speed of 600 r / min, and continuing to keep warm for 4.5 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0155] (4) The intermediate resin M2 prepared in step (3) was added to a grinder and heated to 90°C. The remaining thermoplastic catalyst (10 parts of C-2 and 10 parts of C-5) in step (1) was added to M2 and dispersed for 60 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0156] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0157] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.09 MPa for 40 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130° C. / 3 h+155° C. / 4 h+180° C. / 5 h to obtain a thermoplastic catalyst-modified cyanate ester resin cured product.
[0158] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0159] Example 6
[0160] The method for preparing a thermoplastic catalyst comprises the following steps:
[0161] Under nitrogen, 0.1 mol of diamine monomer (comprising 0.02 mol of 4,6-diaminoresorcinol, 0.06 mol of 2-amino-4-[(3-amino-4-hydroxyphenyl)methyl]phenol, and 0.02 mol of 1,3-bis(4'-aminophenoxy)benzene) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor. The mixture was stirred at room temperature. After the diamine monomer was completely dissolved, 0.05 mol of 4,4'-phenylenedioxydiphthalic anhydride and 0.051 mol of 3,3',4,4'-diphenylether dianhydride were added. Stirring was continued at 8°C for 12 hours to prepare the intermediate polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 160°C. Stirring was continued for 10 hours. A mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The ethanol was heated under reflux in a Soxhlet extractor for two days, and then vacuum-dried at 200°C for two hours, 245°C for three hours, and 300°C for two hours to obtain a pale yellow thermoplastic catalyst, designated C-6. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.65 dL / g, a glass transition temperature of 252°C, and an elongation at break of 45%. The catalyst was crushed to a 500-mesh size.
[0162] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated by weight: 30 parts of 4,4'-methylenebis(2,6-dimethylphenylcyanate), 45 parts of 4,4'-dicyanate diphenylhexafluoropropane, 25 parts of phenolic cyanate resin, thermoplastic catalysts (10 parts of C-3, 10 parts of C-5, 20 parts of C-6), and 10 parts of styrene phenol cyanate;
[0163] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0164] (1) Weigh the raw materials according to the required proportions by weight;
[0165] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of the thermoplastic catalyst (C-5) weighed in step (1) at 160° C. for 2 h under stirring conditions at a speed of 1100 r / min until the component resins are uniformly melted to obtain a prepolymerized intermediate resin M1;
[0166] (3) Cooling the prepolymerized intermediate resin M1 to 100° C., adding 10 parts of the active diluent styrene phenol cyanate weighed in step (1) under stirring at a speed of 700 r / min, and continuing to keep warm for 2 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0167] (4) The intermediate resin M2 prepared in step (3) was added to an internal mixer and heated to 100°C. The remaining thermoplastic catalyst (10 parts of C-3 and 20 parts of C-6) in step (1) was added to M2 and dispersed for 60 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0168] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0169] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 115° C., and degassed under a vacuum pressure of -0.09 MPa for 50 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 135° C. / 3 h+155° C. / 3 h+185° C. / 5 h to obtain a cured thermoplastic catalyst-modified cyanate ester resin.
[0170] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0171] Example 7
[0172] The method for preparing a thermoplastic catalyst comprises the following steps:
[0173] Under nitrogen, 0.1 mol of diamine monomer (containing 0.04 mol of 4,6-diaminoresorcinol and 0.06 mol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor. The mixture was stirred at room temperature. After the diamine monomer was completely dissolved, 0.02 mol of 2,3,3',4'-biphenyltetracarboxylic dianhydride and 0.0825 mol of 3,3',4,4'-biphenyl ether dianhydride were added. Stirring was continued at 5°C for 10 hours to prepare the intermediate polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 180°C. Stirring was continued for 8 hours. A mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was heated under reflux in the ethanol in a Soxhlet extractor for two days and then vacuum-dried at 195°C for 4 hours, 255°C for 3 hours, and 300°C for 1 hour to obtain a pale yellow thermoplastic catalyst, designated C-1. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.85 dL / g, a glass transition temperature of 285°C, and an elongation at break of 43%. The catalyst was crushed to a 500-mesh size.
[0174] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated by weight: 45 parts of 4,4'-dicyanate diphenyl propane, 20 parts of 4,4'-dicyanate diphenyl butane, 35 parts of 2,2-bis(4-cyanate-3,5-dimethylphenyl) propane, thermoplastic catalysts (10 parts of C-5 and 20 parts of C-7), and 10 parts of 4,4'-dicyanate diphenyl ethane;
[0175] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0176] (1) Weigh the raw materials according to the required proportions by weight;
[0177] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of the thermoplastic catalyst (C-5) weighed in step (1) at 150° C. for 4 h at a stirring speed of 1100 r / min until the component resins are uniformly melted to obtain a prepolymerized intermediate resin M1;
[0178] (3) Cooling the prepolymerized intermediate resin M1 to 110° C., adding 10 parts of the active diluent 4,4′-dicyanate diphenylethane weighed in step (1) under stirring at a speed of 800 r / min, and continuing to keep warm for 3 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0179] (4) The intermediate resin M2 prepared in step (3) was added to a high-speed disperser and heated to 90° C. The remaining thermoplastic catalyst (20 parts of C-7) in step (1) was added to M2 and dispersed for 50 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0180] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0181] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.09 MPa for 40 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130° C. / 3 h+155° C. / 4 h+175° C. / 6 h to obtain a thermoplastic catalyst-modified cyanate ester resin cured product.
[0182] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0183] Example 8
[0184] The method for preparing a thermoplastic catalyst comprises the following steps:
[0185] Under nitrogen protection, 0.1 mol of diamine monomer (including 0.03 mol of 4,6-diaminoresorcinol, 0.05 mol of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, and 0.02 mol of 3,3'-dihydroxybenzidine) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor and stirred at room temperature. After the diamine monomer was completely dissolved, 0.05 mol of bisphenol A diether dianhydride, 0.02 mol of 3,3',4,4'-biphenyltetracarboxylic dianhydride and 0.0305 mol of 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride were added, and stirring was continued at 5°C for 12 hours to prepare an intermediate product, a polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 150°C, followed by stirring and reaction for 10 hours. A water separator was then used to separate the distilled xylene and water mixture. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was heated in ethanol and refluxed in a Soxhlet extractor for two days. The precipitate was then vacuum-dried at 200°C for 3 hours, 250°C for 2-4 hours, and 300°C for 2 hours to obtain a pale yellow thermoplastic catalyst, designated C-8. The intrinsic viscosity was 1.1 dL / g, the glass transition temperature was 291°C, and the elongation at break was 37% as measured by an Ubbelohde viscometer. After pulverization in a crusher, the mesh size was 700.
[0186] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated by weight: 40 parts of 4,4'-dicyanatodiphenylmethane, 30 parts of dicyclopentadiene cyanate ester, 30 parts of phenolic cyanate ester, thermoplastic catalyst (5 parts of C-4, 10 parts of C-6, 15 parts of C-8), and 15 parts of 4-cumylphenol cyanate;
[0187] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0188] (1) Weigh the raw materials according to the required proportions by weight;
[0189] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of the thermoplastic catalyst (C-6) weighed in step (1) at 140° C. under stirring conditions at a speed of 1100 r / min for 5 h, until the component resins are uniformly melted to obtain a prepolymerized intermediate resin M1;
[0190] (3) Cooling the prepolymerized intermediate resin M1 to 120° C., adding 15 parts of the active diluent 4-cumylphenol cyanate weighed in step (1) under stirring at a speed of 500 r / min, and continuing to keep warm for 3 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0191] (4) The intermediate resin M2 prepared in step (3) was added to an internal mixer and heated to 90°C. The remaining thermoplastic catalyst (5 parts of C-4 and 15 parts of C-8) in step (1) was added to M2 and dispersed for 60 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0192] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0193] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.09 MPa for 40 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130° C. / 3 h+150° C. / 3 h+180° C. / 4 h to obtain a cured thermoplastic catalyst-modified cyanate ester resin.
[0194] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0195] Example 9
[0196] The method for preparing a thermoplastic catalyst comprises the following steps:
[0197] Under nitrogen protection, 0.1 mol of diamine monomer (which includes 0.04 mol of 4,6-diaminoresorcinol, 0.03 mol of 2-amino-4-[(3-amino-4-hydroxyphenyl)methyl]phenol, 0.03 mol of 9,9-(3-fluoro-4-aminophenyl)fluorene and 500 ml of N,N'-dimethylacetamide) was added to a 1000 ml reactor and stirred at room temperature. After the diamine monomer was completely dissolved, 0.06 mol of hexafluorodianhydride and 0.04125 mol of 3,3',4,4'-biphenyl ether dianhydride were added and stirred at 10 ° C for 12 hours to prepare an intermediate product polyimide acid solution. Continue to add 200 ml of xylene was added, the temperature was raised to 160°C, and the reaction was stirred and continued for 10 hours. Simultaneously, a mixture of distilled xylene and water was separated by a water separator. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The ethanol was heated under reflux in a Soxhlet extractor for two days, and then vacuum-dried at 210°C for 2 hours, 260°C for 2 hours, and 300°C for 2 hours to obtain a pale yellow thermoplastic catalyst, designated C-9. The intrinsic viscosity was 1.2 dL / g, the glass transition temperature was 295°C, and the elongation at break was 29%. After pulverization in a pulverizer, the mesh size was 900.
[0198] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated in parts by weight: 60 parts of 4,4'-dicyanate diphenyl propane, 20 parts of 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-dicyanate, 20 parts of 4,4'-dicyanate diphenyl sulfone, thermoplastic catalyst (4 parts of C-1, 5 parts of C-3, 7 parts of C-5, 5 parts of C-7, 9 parts of C-9), and 8 parts of tert-butylphenol cyanate;
[0199] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0200] (1) Weigh the raw materials according to the required proportions by weight;
[0201] (2) 100 parts of the cyanate resin weighed in step (1) and 4 parts of the thermoplastic catalyst (C-1, 6 parts of C-5) were melt-polymerized at 130° C. under stirring conditions at a speed of 800 r / min for 6 hours, and the prepolymerized intermediate resin M1 was obtained after the component resins were uniformly melted;
[0202] (3) Cooling the prepolymerized intermediate resin M1 to 130° C., adding 8 parts of the active diluent tert-butylphenol cyanate weighed in step (1) under stirring at a speed of 600 r / min, and continuing to keep warm for 5 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0203] (4) The intermediate resin M2 prepared in step (3) was added to a grinder and heated to 80°C. The remaining thermoplastic catalyst (5 parts of C-3, 1 part of C-5, 5 parts of C-7, and 9 parts of C-9) in step (1) was added to M2 and dispersed for 60 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0204] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0205] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.1 MPa for 50 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 135° C. / 3 h+155° C. / 4 h+180° C. / 6 h to obtain a thermoplastic catalyst-modified cyanate ester resin cured product.
[0206] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0207] Example 10
[0208] The method for preparing a thermoplastic catalyst comprises the following steps:
[0209] Under nitrogen protection, 0.1 mol of diamine monomer (including 0.03 mol of 4,6-diaminoresorcinol, 0.02 mol of 2,2-bis(3-amino-4-hydroxyphenyl)propane, 0.02 mol of 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine), 0.02 mol of 4,4'-bis(3-aminophenoxy)diphenyl sulfone, 0.01 mol of m-phenylenediamine and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor and stirred at room temperature. After the diamine monomer was completely dissolved, 0.04 mol of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 0.041 mol of 3,3',4,4'-biphenyl ether dianhydride, 0.02 mol of 3,3',4,4'-Benzophenonetetracarboxylic dianhydride was stirred at 8°C for 12 hours to produce an intermediate polyimide acid solution. 200ml of xylene was then added to the solution, and the temperature was raised to 170°C, with stirring, for 10 hours. A water separator was used to separate the distilled xylene and water mixture. Once the water was removed, a thermoplastic catalyst solution containing pendant hydroxyl groups was obtained. The resin solution was added to 2000ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was heated under reflux in ethanol in a Soxhlet extractor for two days and then vacuum-dried at 200°C for 2 hours, 255°C for 4 hours, and 300°C for 2 hours to obtain a pale yellow thermoplastic catalyst, designated C-10. The intrinsic viscosity was 0.69 dL / g, the glass transition temperature was 287°C, and the elongation at break was 28%. After crushing in a pulverizer, the mesh size was 600.
[0210] The latent thermoplastic catalyst modified cyanate ester is prepared from the following components calculated in parts by weight: 40 parts of 4,4'-dicyanate diphenyl propane, 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-dicyanate diphenyl hexafluoropropane, a thermoplastic catalyst (2 parts of C-1, 5 parts of C-4, 2 parts of C-5, 3 parts of C-8, 8 parts of C-10), and 10 parts of nonylphenol cyanate;
[0211] The preparation method of a latent thermoplastic catalyst modified cyanate ester comprises the following steps:
[0212] (1) Weigh the raw materials according to the required proportions by weight;
[0213] (2) 100 parts of the cyanate resin weighed in step (1) and a thermoplastic catalyst (2 parts of C-1, 5 parts of C-4, and 3 parts of C-8) were melt-polymerized at 165° C. for 1.5 hours under stirring conditions at a speed of 800 r / min until the component resins were uniformly melted to obtain a prepolymerized intermediate resin M1;
[0214] (3) Cooling the prepolymerized intermediate resin M1 to 120° C., adding 10 parts of the active diluent nonylphenol cyanate weighed in step (1) under stirring at a speed of 750 r / min, and continuing to keep warm for 3 hours until the resin has no crystals precipitated at room temperature to obtain the intermediate resin M2;
[0215] (4) The intermediate resin M2 prepared in step (3) was added to an internal mixer and heated to 70°C. The remaining thermoplastic catalyst (2 parts of C-5 and 8 parts of C-10) in step (1) was added to M2 and dispersed for 40 minutes to obtain a uniform resin, which is the modified cyanate ester resin.
[0216] The preparation method of a latent thermoplastic catalyst-modified cyanate ester cured product comprises the following steps:
[0217] 300 g of a latent thermoplastic catalyst-modified cyanate ester resin was placed in a beaker, heated to 120° C., and degassed under a vacuum pressure of -0.09 MPa for 40 min. The latent thermoplastic catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 125° C. / 3 h+155° C. / 3 h+185° C. / 5 h to obtain a cured thermoplastic catalyst-modified cyanate ester resin.
[0218] The properties of the latent thermoplastic catalyst prepared in this example are shown in Table 1, the properties of the cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 2, and the properties of the cured cyanate ester resin modified with the latent thermoplastic catalyst are shown in Table 3.
[0219] Comparative Example 1
[0220] The preparation method of thermoplastic polyimide comprises the following steps:
[0221] Under nitrogen protection, 0.1 mol of diamine monomer (containing 0.07 mol of m-phenylenediamine, 0.03 mol of 2,2'-(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine) and 500 ml of N,N'-dimethylacetamide were added to a 1000 ml reactor and stirred at room temperature. After the diamine monomer was completely dissolved, 0.05 mol of 2,3,3',4'-biphenyltetracarboxylic dianhydride and 0.05125 mol of 3,3',4,4'-biphenyl ether dianhydride were added. Stirring was continued at 5°C for 12 hours to prepare an intermediate polyimide acid solution. 200 ml of xylene was then added to the solution, and the temperature was raised to 160°C. Stirring was continued for 10 hours. A mixture of distilled xylene and water was separated by a water separator. After the water was removed, a thermoplastic polyimide resin solution free of pendant hydroxyl structures was obtained. The resin solution was added to 2000 ml of ethanol to obtain a thermoplastic catalyst precipitate. The precipitate was then heated under reflux in a Soxhlet extractor for two days and then vacuum-dried at 190°C for 3 hours, 245°C for 4 hours, and 300°C for 2 hours to obtain a pale yellow thermoplastic catalyst, designated C-11. An Ubbelohde viscometer revealed an intrinsic viscosity of 0.45 dL / g, a glass transition temperature of 283°C, and an elongation at break of 38%. The catalyst was crushed to a 400-mesh size.
[0222] The thermoplastic polyimide modified cyanate resin is prepared from the following components calculated by weight: 100 parts of 4,4'-dicyanate diphenyl propane, 20 parts of thermoplastic polyimide (C-11), and 10 parts of 4-cumylphenol cyanate;
[0223] The preparation method of thermoplastic polyimide modified cyanate ester comprises the following steps:
[0224] (1) Weigh the raw materials according to the required proportions by weight;
[0225] (2) melt-polymerizing 100 parts of the cyanate resin and 10 parts of thermoplastic polyimide C-11 weighed in step (1) at 140° C. at a stirring speed of 800 r / min for 5 h, until the component resins are uniformly melted to obtain a pre-polymerized intermediate resin M1;
[0226] (3) Cooling the prepolymerized intermediate resin M1 to 110° C., adding 10 parts of the active diluent 4-cumylphenol cyanate weighed in step (1) under stirring at a speed of 200 r / min, and continuing to keep warm for 2 hours until the resin is free of crystals at room temperature to obtain the intermediate resin M2;
[0227] (4) The intermediate resin M2 prepared in step (3) was added to a high-speed disperser and heated to 90° C. The remaining 10 parts of the thermoplastic polyimide C-11 in step 1 were added to M2 and dispersed for 45 minutes to obtain a uniform resin, which is a thermoplastic polyimide-modified cyanate resin.
[0228] The preparation method of thermoplastic polyimide modified cyanate ester cured product comprises the following steps:
[0229] 300 g of thermoplastic polyimide-modified cyanate ester resin was placed in a beaker, heated to 120°C, and degassed at a vacuum pressure of -0.09 MPa for 40 minutes. The thermoplastic polyimide-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130°C / 2h+150°C / 3h+180°C / 5h to obtain a thermoplastic polyimide-modified cyanate ester resin cured product.
[0230] The properties of the thermoplastic polyimide-modified cyanate ester prepared in this embodiment are shown in Table 1, the properties of the thermoplastic polyimide-modified cyanate ester are shown in Table 2, and the properties of the thermoplastic polyimide-modified cyanate ester cured product are shown in Table 3.
[0231] Comparative Example 2
[0232] Nonylphenol as catalyst for modified cyanate ester resin
[0233] The nonylphenol catalyst modified cyanate resin is prepared from the following components calculated by weight: 100 parts of 4,4'-dicyanate diphenyl propane, 20 parts of nonylphenol catalyst, and 10 parts of 4-cumylphenol cyanate;
[0234] The preparation method of nonylphenol catalyst modified cyanate ester resin comprises the following steps:
[0235] (1) Weigh the raw materials according to the required proportions by weight;
[0236] (2) melt-polymerizing the cyanate resin and nonylphenol catalyst weighed in step (1) at a temperature of 130° C. under stirring conditions at a speed of 1000 r / min for 3 hours, until the component resins are uniformly melted to obtain a prepolymerized main resin M;
[0237] (3) The main resin M after prepolymerization is cooled to 110° C., and the active diluent 4-cumylphenol cyanate weighed in step (1) is added under stirring at a speed of 300 r / min, and the temperature is kept for 2 hours. When no crystals are precipitated from the resin at room temperature, a molten uniform resin is finally obtained, which is the modified cyanate resin.
[0238] The preparation method of a nonylphenol catalyst-modified cyanate ester resin cured product comprises the following steps:
[0239] 300 g of nonylphenol catalyst-modified cyanate ester resin was placed in a beaker, heated to 120°C, and degassed at a vacuum pressure of -0.09 MPa for 40 minutes. The nonylphenol catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130°C / 2h+150°C / 3h+180°C / 5h to obtain a nonylphenol catalyst-modified cyanate ester resin cured product.
[0240] The properties of the nonylphenol catalyst modified cyanate resin prepared in this comparative example are shown in Table 2, and the properties of the nonylphenol catalyst modified cyanate resin cured product are shown in Table 3.
[0241] Comparative Example 3
[0242] Phenolic resin as catalyst for modified cyanate ester
[0243] The phenolic resin catalyst modified cyanate resin is prepared from the following components calculated in parts by weight: 100 parts of 4,4'-dicyanate diphenyl propane, 20 parts of phenolic resin catalyst (Mn: 2000-3000), and 10 parts of 4-cumylphenol cyanate;
[0244] The preparation method of phenolic resin catalyst modified cyanate resin is the same as that of Comparative Example 2;
[0245] The preparation method of a phenolic resin catalyst-modified cyanate ester resin cured product comprises the following steps:
[0246] 300 g of phenolic resin catalyst-modified cyanate ester resin was placed in a beaker, heated to 120°C, and degassed at a vacuum pressure of -0.09 MPa for 40 minutes. The phenolic resin catalyst-modified cyanate ester resin was then poured into a mold coated with a release agent and cured according to a heating program of 130°C / 2h+150°C / 3h+180°C / 5h to obtain a phenolic resin catalyst-modified cyanate ester resin cured product.
[0247] The properties of the phenolic resin catalyst modified cyanate resin prepared in this comparative example are shown in Table 2, and the properties of the phenolic resin catalyst modified cyanate resin cured product are shown in Table 3.
[0248] The properties of the thermoplastic catalyst and thermoplastic polyimide in Comparative Example 1 and Examples 1-10 are shown in Table 1.
[0249] Table 1 Performance data of thermoplastic catalysts and thermoplastic polyimides in Comparative Example 1 and Examples 1-10
[0250]
[0251] The properties of the modified cyanate ester resins in Comparative Examples 1, 2, 3 and Examples 1-10 are shown in Table 2;
[0252] Table 2 Performance data of modified cyanate resin in Comparative Examples 1, 2, 3 and Examples 1-10
[0253]
[0254]
[0255] The tensile strength, flexural strength, impact strength, glass transition temperature and thermal decomposition temperature of the modified cyanate ester resin cured products in Comparative Examples 1, 2, 3 and Examples 1-10 are shown in Table 3.
[0256] Table 3: Performance data of modified cyanate ester resin cured products in Comparative Examples 1, 2, 3 and Examples 1-10
[0257]
[0258] Note: “-” indicates that the sample is close to the glass transition temperature of the resin at high temperature and no data was tested.
[0259] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A latent thermoplastic catalyst modified cyanate resin, prepared from the following raw materials in parts by weight: Cyanate resin: 100 parts, thermoplastic catalyst: 15-40 parts, active diluent: 5-15 parts; The thermoplastic catalyst is a thermoplastic polyimide resin containing a side hydroxyl structure in the main chain of the molecule and has a structure shown in Formula I. In formula I, m and n are the number of structural units respectively, m is an integer ≥20, n is an integer ≥0; 20≤m+n≤100, R1 is an aromatic dianhydride monomer, R2 is an aromatic diamine monomer containing a hydroxyl structure, and R3 is an aromatic diamine monomer not containing a hydroxyl structure.
2. The latent thermoplastic catalyst modified cyanate resin according to claim 1, characterized in that: The R1 is one or more of Formula 1-1 to Formula 1-11:
3. The latent thermoplastic catalyst modified cyanate ester resin according to claim 1, characterized in that: The R2 is one or more of Formula 2-1 to Formula 2-6:
4. The latent thermoplastic catalyst modified cyanate ester resin according to claim 1, characterized in that: The R3 is one or more of Formula 3-1 to Formula 3-26:
5. The latent thermoplastic catalyst modified cyanate ester resin according to any one of claims 1 to 4, characterized in that: The thermoplastic catalyst has a logarithmic viscosity of 0.25-1.5 dL / g, a glass transition temperature of 230-300° C., a breaking elongation of ≥20%, and a mesh size of 300-1000 meshes.
6. A method for preparing a latent thermoplastic catalyst modified cyanate ester resin as claimed in any one of claims 1 to 5, comprising the following steps: A) stirring a cyanate resin and a part of a thermoplastic catalyst under heating conditions to perform a prepolymerization reaction to obtain a prepolymerized intermediate resin M1; B) stirring and mixing the prepolymerized intermediate resin and a reactive diluent, and reacting until no crystals are precipitated at room temperature, to obtain an intermediate resin M2; C) Mechanically mixing the remaining thermoplastic catalyst with the intermediate resin M2 to react to obtain a latent thermoplastic catalyst-modified cyanate ester resin.
7. The preparation method according to claim 6, characterized in that: The mass of the part of the thermoplastic catalyst in step A) accounts for 15 to 50% of the total mass of the thermoplastic catalyst; In the step A), the cyanate resin and part of the thermoplastic catalyst are stirred at a speed of 200 to 2000 r / min and kept at a constant temperature of 110 to 170° C. for 1 to 10 hours.
8. The preparation method according to claim 6, characterized in that: The reaction temperature in step B) is 90-150° C. and the reaction time is 1-8 hours; In step B), the stirring speed is 100 to 1500 r / min; The reaction temperature in step C) is 50-100° C. and the reaction time is 30-60 min.
9. Use of the latent thermoplastic catalyst modified cyanate resin as claimed in claim 1 in the fields of aviation, aerospace and electronics.
10. The use according to claim 9, characterized in that: Curing the latent thermoplastic catalyst modified cyanate resin to obtain a modified cyanate resin cured product, which is applied in the fields of aviation, aerospace and electronics; The glass transition temperature of the modified cyanate resin cured product is ≥250°C, the tensile strength of the modified cyanate resin at room temperature is ≥85MPa, the elongation at break is ≥3.5%, and the impact strength is ≥25kJ / m 2 Compared with the tensile strength of the resin at room temperature, the tensile strength retention rate of the resin at 177°C is ≥50%, and the thermal decomposition temperature of 5% is ≥410°C.
Citation Information
Patent Citations
High-temperature endurable active toughener powder used for epoxy resin and preparation method thereof
CN101565504A
Modified cyanate ester resin and preparation method of modified cyanate ester resin
CN105440283A
Cyanate ester resin composition for RTM (resin transfer moulding) process and preparation method thereof
CN106751819A
Synergistic toughened modified cyanate resin and preparation method
CN106810862A
Thermoplastic polyimide resin, preparation method thereof and polyimide composite material
CN112266479A
Cited By
Polyimide modified cyanate ester compound as well as preparation method and application thereof