Thin film packaging material and application thereof

By introducing hydrophilic group-modified hollow micro-nanoparticles into the organic encapsulation layer of the film encapsulation material, the problems of insufficient water-oxygen barrier properties and high dielectric constant in the prior art are solved, and better resistance is achieved Hydrogen oxygen capacity and electrical properties extend the service life of the device.

CN118956079APending Publication Date: 2024-11-15SHANGHAI TIANMA MICRO ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075758.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing thin film packaging technology lacks performance in blocking water and oxygen, and metal oxides and anhydrous metal chloride desiccants are prone to corrosion and have a high dielectric constant, which affects device stability and electrical performance.

Method used

The thin film encapsulation material adopting a laminated structure includes a first inorganic encapsulation layer, an organic encapsulation layer and a second inorganic encapsulation layer, wherein the hollow micro-nanoparticles modified by hydrophilic groups are introduced into the organic encapsulation layer to fix water molecules through hydrogen bonding, thereby enhancing the Water-blocking oxygen capacity and reduce the dielectric constant through the hollow structure.

Benefits of technology

It significantly improves the water-blocking oxygen capacity and electrical performance of thin film packaging materials, reduces the dielectric constant, extends the service life of the device and improves stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956079A_ABST
    Figure CN118956079A_ABST
Patent Text Reader

Abstract

The invention provides a thin film packaging material and application thereof, and belongs to the technical field of photoelectric device packaging. The thin film packaging material comprises a first inorganic packaging layer, an organic packaging layer and a second inorganic packaging layer which are arranged in a stacked mode. The organic packaging layer is arranged between the first inorganic packaging layer and the second inorganic packaging layer; the organic encapsulation layer comprises a polymer matrix and hydrophilic group modified hollow micro-nano particles dispersed in the polymer matrix; the hydrophilic group modified hollow micro-nano particle comprises a hollow micro-nano particle and a hydrophilic group bonded on the surface of the hollow micro-nano particle. According to the thin film packaging material provided by the invention, the hydrophilic group modified hollow micro-nano particles are introduced into the organic packaging layer, so that the water and oxygen resistance of the thin film packaging material is improved, the dielectric constant is reduced, corrosive substances are not generated, and the stability of the thin film packaging material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optoelectronic device packaging, and in particular relates to a thin film packaging material and application thereof. Background Art

[0002] Optoelectronic devices, such as organic light emitting devices (OLED), are widely used in display, lighting and other fields. However, OLED devices will be corroded and damaged by water vapor and oxygen, so they need to be protected from water and oxygen.

[0003] Thin-Film Encapsulation (TFE) is a commonly used OLED device encapsulation technology. The film usually includes a three-layer structure of inorganic encapsulation layer / organic encapsulation layer / inorganic encapsulation layer. Although TFE can block water and oxygen to a certain extent, it still has certain disadvantages, such as short life and limited ability to block water and oxygen, and cannot meet commercial needs under certain circumstances.

[0004] In order to improve the ability of the thin film packaging structure to block water and oxygen, there is a related technology that fills the organic layer with fiber materials. When subjected to external force, the external force is transmitted to the fiber materials, and the fiber materials can absorb higher tensile stress and maintain slight deformation, thereby improving the mechanical properties of the organic layer, preventing the organic layer from cracking due to tension or stress, and blocking the diffusion of water and oxygen inside the organic layer, thereby improving the anti-cracking performance and anti-water and oxygen performance of the thin film packaging structure, and extending the service life of the thin film packaging structure. CN110364640A discloses a packaging structure, which includes at least two inorganic layers and at least one organic layer, and the organic layer is arranged between the inorganic layers; the organic layer includes a cavity-containing microparticle desiccant and / or a pore-containing microparticle desiccant; the cavity-containing microparticle desiccant or the pore-containing microparticle desiccant is any one of metal oxides, anhydrous metal chlorides, silica gel or desiccant composites or a mixture of at least two; the metal oxide is hollow magnesium oxide powder and / or hollow calcium oxide powder; the anhydrous metal chloride is anhydrous calcium chloride and / or anhydrous magnesium chloride. This packaging structure can effectively block water and oxygen to protect OLED devices while preventing the desiccant from absorbing water and expanding, causing the inorganic layer to crack, thereby extending the service life.

[0005] However, the above fiber materials have little effect on improving the water and oxygen barrier performance of the thin film packaging structure; while metal oxides and anhydrous metal chloride desiccants can improve the water and oxygen barrier performance of the thin film packaging structure by absorbing water, they are alkaline or acidic after absorbing water, which can easily corrode the thin film packaging material. Moreover, the dielectric constant of the above materials is relatively high (for example, the relative dielectric constant of MgO is 9.65), which can easily lead to a relatively large dielectric constant of the thin film packaging material. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a thin film packaging material and its application. The thin film packaging material has good water and oxygen barrier ability, low dielectric constant, no corrosive substances, and good stability.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a thin film encapsulation material, the thin film encapsulation material comprising a first inorganic encapsulation layer, an organic encapsulation layer, and a second inorganic encapsulation layer stacked;

[0009] The organic encapsulation layer is disposed between the first inorganic encapsulation layer and the second inorganic encapsulation layer;

[0010] The organic encapsulation layer includes a polymer matrix and hollow micro-nanoparticles modified with hydrophilic groups dispersed in the polymer matrix;

[0011] The hydrophilic group-modified hollow micro-nano particles include hollow micro-nano particles and hydrophilic groups bonded to the surface of the hollow micro-nano particles.

[0012] In a second aspect, the present invention provides a use of the thin film encapsulation material as described in the first aspect, wherein the thin film encapsulation material is used for encapsulation of optoelectronic devices.

[0013] In a third aspect, the present invention provides an electroluminescent device, comprising a substrate, an electroluminescent device located on the substrate, and the thin film encapsulation material as described in the first aspect covering the electroluminescent device.

[0014] In a fourth aspect, the present invention provides a display panel, comprising the electroluminescent device as described in the third aspect.

[0015] Compared with the related art, the present invention has at least the following beneficial effects:

[0016] The thin film encapsulation material provided by the embodiment of the present invention introduces hollow micro-nano particles modified by hydrophilic groups into the organic encapsulation layer. On the one hand, the hydrophilic groups on the surface of the hollow micro-nano particles modified by hydrophilic groups are easy to form hydrogen bonds with the water molecules entering, thereby fixing the water molecules and preventing the water from further diffusing downward. At the same time, the presence of the hollow micro-nano particles modified by hydrophilic groups can also extend the invasion channel of water and oxygen, thereby improving the water-oxygen barrier of the thin film encapsulation material. Moreover, the improvement of the water-oxygen barrier is also conducive to the thinning of the organic encapsulation layer, which is conducive to reducing costs. On the other hand, the hollow micro-nano particles modified by hydrophilic groups are hollow structures with low density. When introduced into the organic encapsulation layer, the number of polarized molecules per unit volume can be reduced, the polarization reaction can be reduced, and the dielectric constant of the thin film encapsulation material can be reduced. The reduction of the dielectric constant helps to improve electrical performance, reduce signal delay, reduce crosstalk interference, reduce energy consumption, etc. In addition, since the hollow micro-nano particles modified by hydrophilic groups fix water molecules through hydrogen bonding, they will not react chemically with water and will not change the material composition of the organic encapsulation layer, so they help to improve the stability of the thin film encapsulation material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A schematic diagram of the structure of a thin film packaging material provided by an embodiment of the present invention;

[0018] Figure 2 A schematic diagram of the structure of an electroluminescent device provided in an embodiment of the present invention;

[0019] The reference numerals in the drawings are: 1 - thin film encapsulation material, 11 - first inorganic encapsulation layer, 12 - organic encapsulation layer, 13 - second inorganic encapsulation layer, 2 - substrate, 3 - electroluminescent device. DETAILED DESCRIPTION

[0020] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below in conjunction with the accompanying drawings. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0021] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0023] First, as Figure 1 As shown, an embodiment of the present invention provides a thin film encapsulation material, comprising a first inorganic encapsulation layer 11, an organic encapsulation layer 12, and a second inorganic encapsulation layer 13 which are stacked;

[0024] The organic encapsulation layer 12 is disposed between the first inorganic encapsulation layer 11 and the second inorganic encapsulation layer 13;

[0025] The organic encapsulation layer 12 includes a polymer matrix and hollow micro-nanoparticles modified with hydrophilic groups dispersed in the polymer matrix;

[0026] The hydrophilic group-modified hollow micro-nano particles include hollow micro-nano particles and hydrophilic groups bonded to the surface of the hollow micro-nano particles.

[0027] In the embodiment of the present invention, hollow micro-nanoparticles modified with hydrophilic groups are introduced into the organic encapsulation layer of the thin film encapsulation material, thereby improving the water and oxygen barrier capability of the thin film encapsulation material and reducing the dielectric constant of the thin film encapsulation material.

[0028] Specifically, in terms of water and oxygen blocking, the hydrophilic groups on the surface of the hollow micro-nanoparticles modified with hydrophilic groups are easy to form hydrogen bonds with the incoming water molecules, thereby fixing the water molecules and preventing the water from further diffusing downward. At the same time, the presence of the hollow micro-nanoparticles modified with hydrophilic groups can also extend the invasion channel of water and oxygen, thereby improving the water and oxygen blocking ability of the thin film encapsulation material. Moreover, the improvement of the water and oxygen blocking ability is also conducive to the thinning of the organic encapsulation layer and the reduction of costs.

[0029] In terms of reducing the dielectric constant, the hollow micro-nanoparticles modified with hydrophilic groups have a hollow structure and low density. Introducing them into the organic encapsulation layer can reduce the number of polarized molecules per unit volume and polarization reactions, thereby reducing the dielectric constant of the thin film encapsulation material. The reduction of the dielectric constant helps to reduce capacitance, increase signal transmission rate, and is conducive to further thinning of the product and improving optical performance.

[0030] In addition, since the hollow micro-nanoparticles modified with hydrophilic groups fix water molecules through hydrogen bonding, they will not chemically react with water and will not change the material composition of the organic encapsulation layer, thus helping to improve the stability of the thin film encapsulation material.

[0031] In summary, the thin film encapsulation material obtained by the embodiment of the present invention has good water and oxygen barrier ability, low dielectric constant and good stability by introducing the hollow micro-nanoparticles modified with hydrophilic groups into the organic encapsulation layer.

[0032] In some embodiments of the present invention, the particle size of the hollow micro-nanoparticles is 100nm-2μm, for example, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 1.2μm, 1.3μm, 1.5μm, 1.6μm, 1.8μm, 2μm, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0033] In the embodiment of the present invention, the particle size of the hollow micro-nano particles is controlled within the above range, which is helpful to obtain a thin film packaging material with good performance. If the particle size of the hollow micro-nano particles is too small, they are prone to agglomeration and difficult to disperse evenly, and the cost is high, the stability is poor, and it is not conducive to packaging; if the particle size of the hollow micro-nano particles is too large, they are easy to settle when preparing the organic packaging layer ink, resulting in uneven dispersion of the hollow micro-nano particles in the organic packaging layer, or clogging the print head when the organic packaging layer is inkjet printed.

[0034] In some embodiments of the present invention, the porosity of the hollow micro-nanoparticles is 30-80%, for example, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, 78% or 80%, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0035] In the embodiment of the present invention, if the porosity of the hollow micro-nano particles is too large, they are easily broken or deformed, resulting in a decrease in the structural stability of the thin film packaging material; if the porosity of the hollow micro-nano particles is too small, their effect on reducing the dielectric constant of the thin film packaging material is relatively weak.

[0036] In some embodiments of the present invention, the relative dielectric constant (ε r )≤4, for example, it can be 4, 3.8, 3.6, 3.5, 3.3, 3.2, 3, 2.8, 2.6, 2.5, 2.3, 2.2, 2, 1.8, 1.5, etc.; preferably ≤2.5. However, the present invention is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0037] In the embodiment of the present invention, hollow micro-nanoparticles with low dielectric constant are selected, which helps to further reduce the dielectric constant of the organic encapsulation layer, thereby further reducing the dielectric constant of the thin film encapsulation material.

[0038] In some embodiments of the present invention, the hollow micro-nanoparticles include one or more of graphene hollow micro-nanoparticles, SiO2 hollow micro-nanoparticles, SiOF hollow micro-nanoparticles, post-pore formation polymer micro-nanoparticles and periodic mesoporous organosilicon (PMO) micro-nanoparticles.

[0039] Among them, post-pore-forming polymers generally refer to a type of porous polymer material, which is characterized by creating or adjusting the pore structure through specific post-processing steps after the polymer network is formed.

[0040] The hollow micro-nanoparticles have a relatively low dielectric constant, such as the ε r <4, ε of SiO2 r <2.5, ε of SiOF r <2.0, ε of Polymers of post-pore formation r <2.0, PMO ε r <2.0. In the embodiment of the present invention, the hollow micro-nano particles are selected to further reduce the dielectric constant of the thin film packaging material.

[0041] In some embodiments of the present invention, the hydrophilic group includes one or more of a hydroxyl group (-OH), a carboxyl group (-COOH), an amino group (-NH2), an amide group (-NH-CO-) and a sulfonic acid group (-SO3H). However, the present invention is not limited thereto, and other conventional hydrophilic groups in the art may also be applicable to the present invention.

[0042] In the embodiments of the present invention, there is no particular limitation on the preparation method of the hollow micro-nano particles modified with hydrophilic groups. Those skilled in the art can use conventional methods to modify the surface of the hollow micro-nano particles with hydrophilic groups, thereby preparing the hollow micro-nano particles modified with hydrophilic groups. As a non-limiting example, the following method can be used in the embodiments of the present invention:

[0043] (1) Optionally, pre-treating the hollow micro-nanoparticles to remove surface impurities and improve their surface activity;

[0044] (2) mixing the pretreated or unpretreated hollow micro-nano particles with a surface modifier containing a hydrophilic group and a solvent to react so that the hydrophilic group in the surface modifier is bonded to the surface of the hollow micro-nano particles;

[0045] (3) Optionally, after the reaction is completed, the solid product is separated, the unreacted surface modifier and by-products are removed by washing, and then dried to obtain pure hydrophilic group-modified hollow micro-nanoparticles.

[0046] Wherein, the pretreatment includes but is not limited to at least one of ultrasonic dispersion and chemical cleaning.

[0047] The surface modifier includes but is not limited to a silane coupling agent, wherein the siloxane group in the silane coupling agent can react with the hydroxyl group or other functional groups on the surface of the hollow micro-nano particles, thereby bonding the hydrophilic group to the surface of the hollow micro-nano particles. As a non-limiting example, when the hydrophilic group to be modified is a hydroxyl group, the silane coupling agent can be hydroxymethyltriethoxysilane; when the hydrophilic group to be modified is an amino group, the silane coupling agent can be 3-aminopropyltrimethoxysilane (APS).

[0048] The solvent and reaction conditions (such as temperature, time, pH value, etc.) described in step (2) need to be selected according to the characteristics of the hydrophilic group and the surface modifier to ensure efficient and uniform surface modification effect. The reaction time can vary from a few hours to 24 hours, and those skilled in the art can select it according to the type of surface modifier and the desired degree of modification. Generally, a longer reaction time helps to ensure that the surface modifier fully reacts with the surface of the hollow micro-nano particles, but too long a time may lead to unnecessary side reactions or decomposition of the surface modifier.

[0049] In some embodiments of the present invention, the volume content of the hollow micro-nanoparticles modified with hydrophilic groups in the organic encapsulation layer is 0.5-30%, for example, 0.5%, 1%, 2%, 3%, 5%, 6%, 8%, 10%, 12%, 13%, 15%, 16%, 18%, 20%, 22%, 23%, 25%, 26%, 28% or 30%, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0050] In the embodiment of the present invention, the volume content of the hollow micro-nanoparticles modified by the hydrophilic group in the organic encapsulation layer is controlled within the above range, which helps to obtain a thin film encapsulation material with good water and oxygen barrier capacity, good mechanical properties, and low dielectric constant. If the content of the hollow micro-nanoparticles modified by the hydrophilic group is too low, it is difficult to play the role of improving the water and oxygen barrier capacity and reducing the dielectric constant, or even has no effect; if the content of the hollow micro-nanoparticles modified by the hydrophilic group is too high, it may destroy the integrity of the polymer matrix of the organic encapsulation layer, resulting in a decrease in the water and oxygen barrier capacity and mechanical strength of the thin film encapsulation material, and may also affect the flatness of the organic encapsulation layer, resulting in an uneven surface of the organic encapsulation layer, affecting subsequent processes.

[0051] In some embodiments of the present invention, the material of the polymer matrix includes acrylic resin and / or epoxy resin. However, the present invention is not limited thereto, and other conventional polymers used for organic encapsulation layers of thin film encapsulation materials in the art may also be applicable to the present invention.

[0052] In some embodiments of the present invention, the thickness of the organic encapsulation layer is 5-17 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm or 17 μm, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0053] In the implementation of the present invention, the organic encapsulation layer needs to have a certain thickness to eliminate the stress generated by the first inorganic encapsulation layer and the second inorganic encapsulation layer, and a lower thickness of the organic encapsulation layer will also reduce the water and oxygen barrier capacity of the thin film encapsulation material; and as the thickness of the organic encapsulation layer increases, it will affect the light extraction efficiency of the product and the subsequent process, and is not conducive to reducing costs and making the display panel thinner. Therefore, considering comprehensively, the thickness of the organic encapsulation layer in the embodiment of the present invention is preferably within the above range.

[0054] In the embodiment of the present invention, there is no particular limitation on the method for forming the organic encapsulation layer. As a non-limiting example, the organic encapsulation layer may be prepared by the following method:

[0055] The hollow micro-nanoparticles modified with hydrophilic groups and conventional ink are mixed evenly to form encapsulation ink; the encapsulation ink is coated on the first inorganic encapsulation layer and cured to form an organic encapsulation layer. Then the second inorganic encapsulation layer is made normally.

[0056] Among them, the conventional ink refers to the ink used to prepare the conventional polymer material organic encapsulation layer, which contains a polymer or a polymer precursor. The polymer is the polymer matrix material in the organic encapsulation layer, and its curing method is drying. The polymer precursor refers to a substance that can form the polymer matrix material after curing, including but not limited to the monomer or oligomer of the polymer. For the polymer precursor, its curing method is a chemical method, such as light curing, thermal curing, in-situ polymerization reaction, etc.

[0057] For the polymer precursor, the packaging ink may also contain components necessary for curing the polymer precursor, such as an initiator, a curing agent, and the like.

[0058] The packaging ink may also contain a dispersant to improve the dispersion uniformity between the components.

[0059] The coating method of the encapsulation ink is preferably inkjet printing.

[0060] In some embodiments of the present invention, the materials of the first inorganic encapsulation layer and the second inorganic encapsulation layer are independently selected from Al2O3, SiN u 、SiO x 、SiO yN z and SnO2, wherein 0<u<2 (for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc.), 0<x<2 (for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc.), 8 or 1.9, etc.), 0<y<2 (for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc.), 0<z<2 (for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc.). However, the present invention is not limited thereto, and other conventional materials for inorganic encapsulation layers of thin film encapsulation materials in the art may also be applicable to the present invention.

[0061] In some embodiments of the present invention, the thickness of the first inorganic encapsulation layer and the second inorganic encapsulation layer is independently 0.1-1.5 μm, for example, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm or 1.5 μm, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0062] The water and oxygen barrier capacity of the thin film encapsulation material is mainly provided by the first inorganic encapsulation layer and the second inorganic encapsulation layer. If the thickness of the first inorganic encapsulation layer and the second inorganic encapsulation layer is too small, the water and oxygen barrier capacity of the thin film encapsulation material will be significantly reduced; and if the thickness of the first inorganic encapsulation layer and the second inorganic encapsulation layer is too large, it is easy to crack due to its own thermal residual stress, and its excessive thickness is not conducive to reducing costs and thinning the display panel. Therefore, the thickness of the first inorganic encapsulation layer and the second inorganic encapsulation layer in the embodiment of the present invention is preferably within the above range.

[0063] In the embodiment of the present invention, there is no special limitation on the method of forming the first inorganic encapsulation layer and the second inorganic encapsulation layer, and those skilled in the art may prepare them by conventional methods, including but not limited to atomic layer deposition (ALD), plasma enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD), etc.

[0064] In a second aspect, the present invention provides a use of the thin film encapsulation material as described in the first aspect, wherein the thin film encapsulation material is used for encapsulation of optoelectronic devices.

[0065] Thirdly, Figure 2 As shown, the present invention provides an electroluminescent device, which includes a substrate 2, an electroluminescent device 3 located on the substrate 2, and a thin film encapsulation material 1 as described in the first aspect and covering the electroluminescent device 3.

[0066] The electroluminescent device 3 includes but is not limited to LED, OLED, QLED and the like.

[0067] The electroluminescent device provided by the embodiment of the present invention includes the thin film encapsulation material as described in the first aspect, and thus has the same technical effect as the thin film encapsulation material, which will not be described in detail herein.

[0068] In a fourth aspect, the present invention provides a display panel, comprising the electroluminescent device as described in the third aspect.

[0069] The display panel provided by the embodiment of the present invention includes the thin film encapsulation material as described in the first aspect, and thus has the same technical effect as the thin film encapsulation material, which will not be described in detail herein.

[0070] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention will be further described in detail in conjunction with the embodiments below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its applications. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0071] If no specific techniques or conditions are specified in the examples, the conventional techniques or conditions in the art, or the techniques or conditions described in the literature, or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0072] Preparation Example 1

[0073] This preparation example prepares a hydroxyl-modified graphene hollow micro-nanoparticle, and the method is as follows:

[0074] (1) 1 g of graphene oxide (GO, purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.) was dispersed in 500 mL of deionized water to form a suspension, and then appropriate amounts of NaOH and H2O2 were added and reacted at room temperature for 3 h to form graphene oxide with hydroxyl groups (denoted as GO-OH).

[0075] (2) Preparation of PMMA / GO-OH colloidal particles (PMMA:GO = 96:4, wt / wt): 1.0 mg / mL GO-OH solution was gradually added to 1.0 wt% PMMA solution and stirred vigorously for 1.5 h to form PMMA / GO-OH colloidal particles (GO-OH was wrapped on the PMMA surface).

[0076] (3) PMMA / GO-OH colloidal particles were mixed with aniline monomer, where the mass ratio of GO-OH to aniline monomer was 1:7, and stirred at 5 °C for 30 min. Then, ammonium persulfate solution as an oxidant was slowly added and stirred for 24 h.

[0077] (4) The reacted material is filtered to remove unreacted aniline monomer and oxidant, and then thoroughly washed with deionized water and ethanol.

[0078] (5) The sample obtained in the previous step was immersed in chloroform for 4 h to etch away the PMMA core to obtain GO-OH hollow micro-nanoparticles.

[0079] (6) Using a reducing agent, glucose, to chemically reduce the GO-OH hollow micro-nanoparticles to obtain hydroxyl-modified reduced graphene oxide (rGO) hollow micro-nanoparticles, which are then washed multiple times with deionized water and ethanol, and dried to obtain pure hydroxyl-modified graphene hollow micro-nanoparticles. 50 The particle size is 0.4 μm and the porosity is 50%.

[0080] In this preparation example, step (1) is not performed, and GO is used instead of GO-OH in step (2), thereby preparing unmodified graphene hollow micro-nanoparticles.

[0081] Preparation Example 2

[0082] This preparation example prepares a carboxyl-modified SiO2 hollow nanoparticle as follows:

[0083] (1) 0.5 mL of tetraethoxysilane (TEOS) was added to a mixed solution of 25.5 mL of water and 15.0 mL of ethanol, and then 0.08 g of hexadecyltrimethylammonium bromide (CTAB) was added. 0.5 mL of ammonia water was added, and the pH value was raised to 10 and maintained until the reaction was completed. The mixture was stirred at room temperature for 3 hours.

[0084] (2) The product was separated by centrifugation, washed with deionized water and ethanol, and then calcined at 200°C for 6 hours and then at 600°C for 6 hours to obtain hollow silica microspheres.

[0085] (3) The hollow silica microspheres were evenly dispersed in the solvent ethanol, and then 11% of the mass of the hollow silica microspheres was added with a carboxyl-containing silane coupling agent 3-(trimethoxysilyl) propionic acid, and the mixture was reacted at 90° C. for 6 hours.

[0086] (4) After the reaction is completed, the modified microspheres are separated from the unreacted coupling agent by centrifugation, and then washed with an appropriate solvent to remove the residue, and finally dried to obtain carboxyl-modified SiO2 hollow micro-nanoparticles. 50 The particle size is 100 nm and the porosity is 60%.

[0087] In this preparation example, the hollow silica microspheres prepared in step (2) are unmodified SiO2 hollow nanoparticles.

[0088] Preparation Example 3

[0089] This preparation example prepares an amide-modified SiO2 hollow nanoparticle as follows:

[0090] Prepare hollow silica microspheres in the same manner as steps (1) and (2) of Example 2;

[0091] (3) The hollow silica microspheres are evenly dispersed in the solvent ethanol, and then 3-aminopropyltriethoxysilane (APTES) (10% by mass of the hollow silica microspheres), 0.3% of the catalyst N-(3-dimethylaminopropyl)-N'-ethylcarbonyldiimidamide (EDC) and 0.2% of the catalyst N-hydroxysuccinimide (NHS) are added, and the mixture is reacted at 90°C for 6 hours.

[0092] (4) After the reaction is completed, the nanoparticles are separated by centrifugation, washed with an appropriate solvent to remove unreacted raw materials and by-products, and then dried to obtain amide-modified SiO2 hollow nanoparticles. 50 The particle size is 100 nm and the porosity is 60%.

[0093] Preparation Example 4

[0094] This preparation example prepares a sulfonic acid group-modified hollow mesoporous SiO2 nanoparticle as follows:

[0095] (1) Synthesis of hollow mesoporous silica (HMS) nanoparticles (hard template method):

[0096] 1) L-serine-coated magnetic nanoparticles (L-ser@MNPs) were used as solid templates. The solid templates were added into a mixed solution of ethanol (3 mL) and deionized water (60 mL) containing 0.125 g of hexadecyltrimethylammonium chloride, stirred at 80 °C for 1 h, and the pH was adjusted to 10 with NH4OH.

[0097] 2) Add 50 μL of tetraethoxysilane (TEOS) to the mixture and stir for 20 h to form an intermediate product.

[0098] 3) The intermediate product was collected by centrifugation, washed with deionized water, and then stirred in methanol containing 2 mL of hydrochloric acid overnight to remove the template. The solid product was collected by centrifugation, washed with deionized water several times, and finally freeze-dried to obtain HMS nanoparticles.

[0099] (2) Synthesis of PSS (poly styrene sulfonate) modified HMS nanoparticles:

[0100] 1) Disperse 0.1 g of HMS nanoparticles in 50 mL of toluene and stir under a nitrogen atmosphere;

[0101] 2) 48 μL (0.2 mmol) of 3-(trimethoxysilyl)propyl methacrylate (TMPMA) was added and refluxed for 24 hours to generate silanized HMS nanoparticles.

[0102] 3) The silanized HMS nanoparticles were collected by centrifugation and washed with toluene, ethanol and deionized water in sequence.

[0103] 4) The product was redispersed in 5 mL of deionized water, 70 μL of an acetone solution of AIBN (15% w / v) was added at 70° C., and stirred for 10 minutes to initiate polymerization; then 0.2072 g (1 mmol) of sodium 4-vinylbenzenesulfonic acid (Na-VBS) was added to 5 mL of deionized water and directly added to the above reaction solution.

[0104] 5) The polymerization reaction was terminated by adding cold methanol after 20 hours to produce PSS-modified HMS nanoparticles (PSS@HMS).

[0105] 6) PSS@HMS was collected by centrifugation, soaked in 0.1 M HCl solution overnight, then washed with deionized water several times, and dried with a freeze dryer to obtain sulfonic acid group-modified hollow mesoporous SiO2 nanoparticles, D 50 The particle size is 100 nm and the porosity is 30%.

[0106] Example 1

[0107] This embodiment provides an organic electroluminescent device, and its structural schematic diagram is as follows Figure 2 As shown, it includes a substrate 2, an electroluminescent device 3 located on the substrate 2, and a thin film encapsulation material 1 covering the electroluminescent device 3;

[0108] The thin film encapsulation material 1 includes a first inorganic encapsulation layer 11, an organic encapsulation layer 12 and a second inorganic encapsulation layer 13 which are stacked in sequence in a direction away from the electroluminescent device 3;

[0109] The material of the first inorganic encapsulation layer 11 is SiO y N z , 0<y<2, 0<z<2; thickness is 800nm;

[0110] The organic encapsulation layer 12 includes an acrylic resin matrix and hydroxyl-modified graphene hollow micro-nanoparticles prepared in Preparation Example 1. The volume content of the hydroxyl-modified graphene hollow micro-nanoparticles in the organic encapsulation layer 12 is 15%, and the thickness of the organic encapsulation layer 12 is 10 μm.

[0111] The material of the second inorganic encapsulation layer 13 is SiN u , 0<u<2; thickness is 800nm;

[0112] The electroluminescent device 3 is an OLED device.

[0113] In this embodiment, the preparation method of the organic electroluminescent device is as follows:

[0114] S1: preparing OLED devices on a substrate;

[0115] S2: Using PECVD method, a layer of SiO is deposited on the surface of OLED device. x N y , with a thickness of 800 nm, as the first inorganic encapsulation layer 11;

[0116] S3: The hydroxyl-modified graphene hollow micro-nanoparticles prepared in Preparation Example 1 (the added amount is controlled so that the volume content in the organic encapsulation layer 12 is 15%), the dispersant (the content in the encapsulation ink is 0.1wt%), and the commercially available acrylic resin ink (S150 of Xi'an Simoway New Materials Co., Ltd.) are mixed evenly to form an encapsulation ink, and then the encapsulation ink is inkjet printed on the surface of the first inorganic encapsulation layer 11. After the encapsulation ink is leveled, ultraviolet light curing is performed to form an organic encapsulation layer 12 with a thickness of 10 μm;

[0117] S4: Using PECVD method, a layer of SiN is deposited on the surface of the organic encapsulation layer 12 u , with a thickness of 800 nm, as the second inorganic encapsulation layer 13, to obtain the organic electroluminescent device.

[0118] Example 2

[0119] This embodiment provides an organic electroluminescent device, which is different from the embodiment 1 only in that:

[0120] The thickness of the first inorganic encapsulation layer 11 is 100 nm;

[0121] The organic encapsulation layer 12 includes an acrylic resin matrix and carboxyl-modified SiO2 hollow nanoparticles prepared in Preparation Example 2. The volume content of the carboxyl-modified SiO2 hollow nanoparticles in the organic encapsulation layer 12 is 0.5%, and the thickness of the organic encapsulation layer 12 is 5 μm.

[0122] The thickness of the second inorganic encapsulation layer 13 is 100 nm.

[0123] Example 3

[0124] This embodiment provides an organic electroluminescent device, which is different from the embodiment 1 only in that:

[0125] The thickness of the first inorganic encapsulation layer 11 is 1 μm;

[0126] The organic encapsulation layer 12 includes an epoxy resin matrix and amide-modified SiO2 hollow nanoparticles prepared in Preparation Example 3, the volume content of the amide-modified SiO2 hollow nanoparticles in the organic encapsulation layer 12 is 10%, and the thickness of the organic encapsulation layer 12 is 12 μm; in the step of preparing the organic encapsulation layer 12, the commercially available acrylic resin ink is replaced with a commercially available epoxy resin ink (FEI-510 of Hangzhou Foster Applied Materials Co., Ltd.);

[0127] The thickness of the second inorganic encapsulating layer 13 is 1 μm.

[0128] Example 4

[0129] This embodiment provides an organic electroluminescent device, which is different from the embodiment 1 only in that:

[0130] The material of the first inorganic encapsulation layer 11 is Al2O3, and the thickness is 1.5 μm;

[0131] The organic encapsulation layer 12 includes an epoxy resin matrix and hollow mesoporous SiO2 nanoparticles modified with sulfonic acid groups prepared in Preparation Example 4. The volume content of the hollow mesoporous SiO2 nanoparticles modified with sulfonic acid groups in the organic encapsulation layer 12 is 30%, and the thickness of the organic encapsulation layer 12 is 17 μm.

[0132] The material of the second inorganic encapsulation layer 13 is Al 2 O 3 , and the thickness is 1.5 μm.

[0133] Comparative Example 1

[0134] This comparative example provides an organic electroluminescent device, which is different from Example 1 only in that the hydroxyl-modified graphene hollow micro-nanoparticles in the organic encapsulation layer 12 are replaced by unmodified graphene hollow micro-nanoparticles.

[0135] Comparative Example 2

[0136] This comparative example provides an organic electroluminescent device, which is different from Example 2 only in that the carboxyl-modified SiO2 hollow nanoparticles in the organic encapsulation layer 12 are replaced by unmodified SiO2 hollow nanoparticles.

[0137] Comparative Example 3

[0138] This comparative example provides an organic electroluminescent device, which is different from Example 3 only in that the amide-modified SiO2 hollow nanoparticles in the organic encapsulation layer 12 are replaced by unmodified SiO2 hollow nanoparticles.

[0139] Comparative Example 4

[0140] This comparative example provides an organic electroluminescent device, which is different from Example 4 only in that the sulfonic acid group-modified hollow mesoporous SiO2 nanoparticles in the organic encapsulation layer 12 are replaced by unmodified hollow mesoporous SiO2 nanoparticles.

[0141] Comparative Example 5

[0142] This comparative example provides an organic electroluminescent device, which is different from Example 1 only in that the hydroxyl-modified graphene hollow micro-nanoparticles in the organic encapsulation layer 12 are replaced by MgO nanoparticles (D 50 Particle size 50nm, purchased from Shanghai Yaotian New Material Technology Co., Ltd.)

[0143] This comparative example provides an organic electroluminescent device, which is different from Example 1 only in that the organic encapsulation layer 12 does not contain hydroxyl-modified graphene hollow micro-nanoparticles, that is, the layer is composed of an acrylic resin matrix.

[0144] It should be noted that, in the organic electroluminescent devices provided in the above-mentioned embodiments and comparative examples, the parts other than the thin film encapsulation material are the same.

[0145] Performance Testing

[0146] The water-oxygen barrier properties and dielectric constants of the organic encapsulation layer materials in the above embodiments and comparative examples were tested, and the testing method is as follows:

[0147] 1. Water and oxygen barrier properties:

[0148] Test device: 85℃, 85RH% constant temperature and humidity oven.

[0149] Evaluation materials: Metals that react with water and corrode: Calcium; Metals that are impermeable to water vapor: Ag.

[0150] Preparation of samples for water vapor barrier evaluation: Using a vacuum evaporation device, 10 mm × 10 mm metal calcium (thickness of 100 nm) was evaporated on white glass through a mask. Then an organic encapsulation layer (thickness of 10 μm) was printed, wherein the materials of the organic encapsulation layer were the same as those of the embodiment and the comparative example, and then metal Ag (thickness of 100 nm) that is not easily penetrated by water was evaporated, and then UV glue and a glass cover were used for sealing; thus, a sample for testing water and oxygen barrier performance was obtained.

[0151] Then, the samples were stored in a constant temperature and humidity oven at 85°C and 85 RH% for 12h, 24h, and 48h respectively. The percentage of the metal calcium corrosion area to the metal calcium vapor deposition area of ​​10mm×10mm was calculated, and the water vapor barrier properties were evaluated according to the following standards:

[0152] Level 1: The area where metal calcium corrosion occurs accounts for s<1%;

[0153] Level 2: The area where metal calcium corrosion occurs is s1%≤s<4%;

[0154] Level 3: The area where metal calcium corrosion occurs is 4%≤s<10%;

[0155] Level 4: The area where metal calcium corrosion occurs accounts for s≥10%.

[0156] 2. Dielectric constant:

[0157] Test equipment: Impedance analyzer and SME (Scanning Electron Microscope).

[0158] Evaluation materials: A metal first electrode was evaporated on white glass, followed by printing an organic encapsulation layer (thickness of 10 μm), wherein the materials of the organic encapsulation layer were the same as those of the embodiment and the comparative example, and then a second electrode was evaporated (the materials of the first electrode and the second electrode were both Ag). Then, an impedance analyzer was used to perform a capacitance test at a frequency of 100 kHz; then, a SEM was used to test the sample thickness, and the relative dielectric constant was calculated according to the following formula.

[0159]

[0160] Among them, ε r is the relative dielectric constant of the sample; ε0 is the vacuum dielectric constant, which is approximately 8.854187817×10 -12 F / m; C is the sample capacitance, S is the area of ​​the electrode; d is the sample thickness.

[0161] Level 1: ε r <2.3;

[0162] Level 2: 2.3 ≤ ε r <2.4;

[0163] Level 3: 2.5 ≤ ε r <2.6;

[0164] Level 4: 2.6 ≤ ε r <2.7;

[0165] Level 5: 2.7 ≤ ε r <2.8;

[0166] Level 6: Epsilon r >2.8.

[0167] 3. Optical performance:

[0168] Test equipment: UV-visible spectrometer;

[0169] Evaluation materials: An organic encapsulation layer (thickness of 10 μm) was printed on a white glass surface, wherein the materials of the organic encapsulation layer were the same as those in the embodiment and the comparative example, and the transmittance (T%) within the wavelength range of 380 nm-780 nm was tested using an ultraviolet-visible spectrometer.

[0170] Level 1: T%>98%;

[0171] Level 2: 98% ≤ T% ≤ 96%;

[0172] Level 3: T%<96%.

[0173] The results of the above performance tests are shown in Table 1 below.

[0174] Table 1

[0175]

[0176]

[0177] It can be seen from the performance data in Table 1 that, compared with Comparative Examples 1-4, the organic encapsulation layers in Examples 1-4 not only have significantly improved water and oxygen barrier capabilities, but also maintain a stable dielectric constant, indicating that the water and oxygen barrier capabilities of the thin film encapsulation materials can be effectively improved by modifying the hollow micro-nanoparticles with hydrophilic groups and introducing them into the organic encapsulation layer.

[0178] Compared with Example 1, the organic encapsulation layer in Comparative Example 6 does not contain hollow micro-nanoparticles, and the water-oxygen barrier performance and dielectric constant of the organic encapsulation layer are significantly improved, indicating that by introducing hollow micro-nanoparticles modified with hydrophilic groups into the organic encapsulation layer, the dielectric constant of the organic encapsulation layer can be effectively reduced, thereby reducing the dielectric constant of the thin film encapsulation material.

[0179] Compared with Example 1, Comparative Example 5 uses MgO nanoparticles with water absorption capacity instead of hydroxyl-modified graphene hollow micro-nanoparticles. Although the water and oxygen barrier capacity of the formed organic encapsulation layer is equivalent to that of Example 1, the dielectric constant is significantly increased.

[0180] The above description is only a specific embodiment of the present disclosure, so that those skilled in the art can understand or implement the present disclosure. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure will not be limited to the embodiments described herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A thin film packaging material, characterized in that: The thin film encapsulation material comprises a first inorganic encapsulation layer, an organic encapsulation layer and a second inorganic encapsulation layer which are stacked; The organic encapsulation layer is disposed between the first inorganic encapsulation layer and the second inorganic encapsulation layer; The organic encapsulation layer includes a polymer matrix and hollow micro-nanoparticles modified with hydrophilic groups dispersed in the polymer matrix; The hydrophilic group-modified hollow micro-nano particles include hollow micro-nano particles and hydrophilic groups bonded to the surface of the hollow micro-nano particles.

2. The thin film encapsulation material according to claim 1, characterized in that: The particle size of the hollow micro-nano particles is 100nm-2μm; and / or, the porosity of the hollow micro-nanoparticles is 30-80%; And / or, the relative dielectric constant of the hollow micro-nanoparticles is ≤4, preferably ≤2.

5.

3. The thin film encapsulation material according to claim 1 or 2, characterized in that: The hollow micro-nanoparticles include one or more of graphene hollow micro-nanoparticles, SiO2 hollow micro-nanoparticles, SiOF hollow micro-nanoparticles, post-pore-forming polymer micro-nanoparticles and periodic mesoporous organosilicon micro-nanoparticles.

4. The thin film encapsulation material according to claim 1 or 2, characterized in that: The hydrophilic group includes one or more of a hydroxyl group, a carboxyl group, an amino group, an amide group and a sulfonic acid group.

5. The thin film encapsulation material according to claim 1 or 2, characterized in that: The volume content of the hollow micro-nano particles modified with hydrophilic groups in the organic encapsulation layer is 0.5-30%.

6. The thin film encapsulation material according to claim 1, characterized in that: The material of the polymer matrix includes acrylic resin and / or epoxy resin.

7. The thin film encapsulation material according to claim 1, characterized in that: The thickness of the organic encapsulation layer is 5-17 μm.

8. The thin film encapsulation material according to claim 1, characterized in that: The materials of the first inorganic encapsulation layer and the second inorganic encapsulation layer are independently selected from Al2O3, SiN u 、SiO x 、SiO y N z and SnO2, wherein 0<u<2, 0<x<2, 0<y<2, 0<z<2.

9. The thin film encapsulation material according to claim 1, characterized in that: The thickness of the first inorganic encapsulating layer and the second inorganic encapsulating layer are each independently 0.1-1.5 μm.

10. An application of the thin film encapsulation material according to any one of claims 1 to 9, characterized in that: The thin film packaging material is used for packaging optoelectronic devices.

11. An electroluminescent device, characterized in that: The electroluminescent device comprises a substrate, an electroluminescent device located on the substrate, and a thin film encapsulation material according to any one of claims 1 to 9 covering the electroluminescent device.