Resin matrix glass fiber reinforced plastic and preparation method thereof
By combining dextran with modified epoxy resin and polyurethane resin, combining E-type and C-type glass fibers, a resin mesh structure is formed, which solves the aging and local affinity of glass fiber reinforced plastics in high temperature, chemical media and high humidity environments. The force problem improves the toughness and stability of the material and simplifies the manufacturing process.
Patent Information
- Application Number
- CN202411333177.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Glass fiber reinforced plastic aging when exposed to ultraviolet rays, high temperatures or chemical media, resulting in deterioration of material properties and shortening of life, and is prone to fragility when local stress is concentrated, and the manufacturing process is complex, which increases production costs and technical requirements.
Using modified epoxy resin, polyurethane resin and dextran, combined with E-type and C-type glass fibers, a resin mesh structure is formed through specific preparation methods, which enhances the toughness and wear resistance of the material and is subjected to local stress. Stay stable when concentrated.
It significantly improves the toughness, strength and wear resistance of glass fiber reinforced plastics, enhances its stability in high temperature, chemical media and high humidity environments, simplifies manufacturing processes, and reduces production costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass fiber reinforced plastics, and in particular to a glass fiber reinforced plastic and a preparation method thereof. Background Art
[0002] Glass fiber reinforced plastic is a composite material with a wide variety of products and good performance. Its development background can be traced back to the mid-20th century. It is mainly composed of glass fiber and resin matrix; glass fiber is used as a reinforcing material to provide high strength and stiffness. E-type glass fiber is usually used, and its characteristics include excellent tensile strength and stiffness. The resin matrix is used as a binder and environmental protection layer for the glass fiber. Thermosetting resins such as epoxy resins, polyester resins or phenolic resins are usually selected. These resins can provide good corrosion resistance and chemical resistance. Overall, glass fiber reinforced plastics continue to develop and have been widely used in fields such as construction, transportation, energy and electronics.
[0003] Although glass fiber reinforced plastics currently perform well under many environmental conditions, their durability and long-term stability are still facing challenges. In particular, the resin matrix and fibers of glass fiber reinforced plastics exposed to ultraviolet rays, high temperatures or chemical media may age, resulting in degradation of material performance and shortened life. This is a potential problem for long-term use or outdoor applications; although glass fiber itself has high strength and stiffness, glass fiber reinforced plastics are more prone to fragmentation and fracture than metal materials, especially under impact or localized force concentration, which limits its application under certain high-load conditions; the resin matrix in glass fiber reinforced plastics has a certain degree of water absorption, especially in high humidity or humid environments, which will lead to a decrease in the physical properties of the material such as strength and stiffness, and even cause corrosion problems; compared with traditional materials, the manufacturing process of glass fiber reinforced plastics is more complicated, involving multiple steps such as the preparation of prepregs, the molding and curing of composite materials. This not only increases production costs, but also requires higher technical requirements and equipment investment.
[0004] Therefore, it is an urgent problem to invent a glass fiber reinforced plastic that has strong environmental tolerance, simple process and certain toughness to ensure excellent stability under conditions of local force concentration.
[0005] In view of the above technical defects, a solution is now proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a glass fiber reinforced plastic and a preparation method thereof, wherein the glass fiber reinforced plastic has strong environmental tolerance, simple process and certain toughness to ensure excellent stability under the condition of local force concentration.
[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a glass fiber reinforced plastic comprises the following components in percentage: modified epoxy resin 25%-30%, polyurethane resin 10%-15%, hardener 5%-15%, glass fiber 30%-50%, initiator 3%-5%, antioxidant 0.5%-3%, light stabilizer 0.5%-3% and filler 5%-10%.
[0008] Furthermore, considering that the combined resin of epoxy resin and polyurethane resin cross-linking and curing still lacks certain strength and toughness, the present invention provides a method for modifying epoxy resin. The use of dextran to modify epoxy resin can significantly enhance its toughness, strength and wear resistance. Dextran is a polysaccharide compound, usually extracted from plants or microorganisms, and has good compatibility.
[0009] The preparation method of the modified epoxy resin comprises the following steps:
[0010] A1: Add epoxy resin and glacial acetic acid into deionized water, heat in an oil bath pot equipped with a thermometer and a magnetic stirrer, stir and react for 30 min at a temperature of 100-120°C and a stirring rate of 500-600 rpm. After complete dissolution, adjust the temperature to 45-60°C, set the stirring rate to 300-400 rpm, and stir for 2 h to obtain intermediate A;
[0011] A2: Add dextran and organosilane coupling agent to intermediate A, use a flask equipped with a stirrer and a thermometer, tilt the flask mouth at 45 degrees, heat the bottom with an alcohol lamp, stir and react for 30 minutes at a temperature of 30-45°C and a stirring rate of 400-600rpm, then use a serpentine tube and condensed water to reflux the product, and reflux for 5-6 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, wash the filter cake with deionized water for 3-5 times, and then place it in a vacuum drying oven and dry it at a temperature of 80-85°C for 3-5 hours to obtain intermediate B;
[0012] A3: The intermediate B is transferred to a distillation tower, and the bottom product of the distillation is collected after distillation for 3-5 hours; the bottom product of the distillation is transferred to room temperature and cooled for 1-2 hours to obtain a modified epoxy resin.
[0013] Furthermore, the epoxy resin is one of bisphenol A epoxy resin, bisphenol F epoxy resin, propylene oxide resin and phenolic resin. The present invention preferably uses bisphenol A epoxy resin, which contains more hydroxyl groups and has excellent polarity and chemical activity.
[0014] Furthermore, the glass fiber is E-type glass fiber and C-type glass fiber, wherein the ratio of the two is 1:1, the E-type glass fiber has higher electrical insulation performance and thermal stability, and the C-type glass fiber has stronger chemical stability and corrosion resistance; a 1:1 mixture of the two can make the glass fiber reinforced plastic have stronger heat resistance and corrosion resistance.
[0015] Furthermore, the hardener is one of tributyl phosphate and phthalic acid diester; the initiator is one of stearamide and imidazole; the antioxidant is one of phenylene sulfide and dimethylbenzene; the light stabilizer is one of p-hydroxybenzoic acid methyl ester and dibenzofuran; the filler is one or more of silicate, calcium carbonate, aluminum hydroxide and silica powder.
[0016] A method for preparing a resin-based glass fiber reinforced plastic comprises the following steps:
[0017] S1: Preparation of modified epoxy resin;
[0018] S2: Mix the resin matrix modified epoxy resin and the tough filler polyurethane resin in a reaction kettle, stir at 45-65°C and 800-1200rpm for 30min, then add the initiator, stir at 65-70°C and 800-1200rpm for 120min, then vacuum filter and wash the filter cake to obtain a tough resin mixture;
[0019] S3: adding the hardener to the tough resin mixture, placing the reactor in a gas bath, steam heating to 65-90°C for 15 minutes, setting a magnetic rotor stirrer at the bottom of the reactor, setting the speed to 1000-1600 rpm and stirring for 30 minutes to obtain a hardened tough resin mixture;
[0020] S4: Add filler, light stabilizer and antioxidant into the reactor, adjust the temperature of the air bath to 55-60°C, set the speed of the magnetic rotor stirrer to 600-800rpm, stir at low speed for 2h to evenly disperse the filler in the mixture matrix, then add glass fiber into the reaction system, transfer the reactor to the oil bath, set the temperature of the oil bath to 160-180°C, set the speed of the magnetic rotor stirrer to 300-500rpm and stir for 2h;
[0021] S5: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 0.5-1h to obtain a glass fiber reinforced plastic.
[0022] In summary, due to the adoption of the above technical scheme, the beneficial effects of the present invention are as follows: the present invention uses dextran to modify epoxy resin to significantly enhance its toughness, strength and wear resistance. Dextran is a polysaccharide compound, usually extracted from plants or microorganisms, and has good compatibility. The modified epoxy resin and the polyurethane resin are combined to form a resin network structure, which has strong tensile strength and impact resistance. At the same time, E-type glass fiber and C-type glass fiber are used, wherein the ratio of the two is 1:1, and the E-type glass fiber has high electrical insulation performance and thermal stability, and the C-type glass fiber has strong chemical stability and corrosion resistance; the 1:1 mixing of the two can make the glass fiber reinforced plastic have strong heat resistance and corrosion resistance. The present invention can still have excellent stability under the condition of local force concentration, so as to solve the problem that the existing glass fiber reinforced plastic is easy to break and fracture under the condition of impact or local force concentration, and has poor durability and corrosion resistance. DETAILED DESCRIPTION
[0023] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0024] The experimental methods in the following examples, unless otherwise specified, are conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials and reagents used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0025] Example 1
[0026] 1: Add 200g of bisphenol A epoxy resin and 2L of glacial acetic acid to deionized water, heat in an oil bath pot equipped with a thermometer and a magnetic stirrer, stir and react for 30min at a temperature of 100-120°C and a stirring rate of 500-600rpm. After complete dissolution, adjust the temperature to 45-60°C, set the stirring rate to 300-400rpm, and stir for 2h to obtain intermediate A;
[0027] 2: Add 100g of dextran and 12g of organosilane coupling agent to intermediate A, use a flask equipped with a stirrer and a thermometer, tilt the flask mouth at 45° and heat the bottom with an alcohol lamp, stir and react for 30min at a temperature of 30-45°C and a stirring rate of 400-600rpm, then use a serpentine tube and condensed water to heat and reflux the product, heat and reflux for 5-6h, cool the reaction product to room temperature after the reaction, then vacuum filter, wash the filter cake with deionized water for 3-5 times, then place it in a vacuum drying oven, and dry it at a temperature of 80-85°C for 3-5h to obtain intermediate B;
[0028] 3: Transfer intermediate B to a distillation tower, control the pressure of the distillation tower to 0.5 atm, and collect the distillation bottom product after distillation for 3-5 hours; transfer the distillation bottom product to room temperature and cool it for 1-2 hours to obtain 285g of modified epoxy resin.
[0029] Table 1, reagent parameters used in Example 1
[0030]
[0031]
[0032] Example 2
[0033] 1: Add 200g of propylene oxide resin and 2L of glacial acetic acid into deionized water, heat in an oil bath pot equipped with a thermometer and a magnetic stirrer, stir and react for 30min at a temperature of 100°C and a stirring rate of 500rpm. After complete dissolution, adjust the temperature to 45°C, set the stirring rate to 400rpm, and stir for 2h to obtain intermediate A;
[0034] 2: Add 100g of dextran and 12g of organosilane coupling agent to intermediate A, use a flask equipped with a stirrer and a thermometer, tilt the flask mouth at 45° and heat the bottom with an alcohol lamp, stir and react for 30min at a temperature of 45°C and a stirring rate of 400rpm, then use a serpentine tube and condensed water to reflux the product, reflux for 6h, cool the reaction product to room temperature after the reaction, then vacuum filter, wash the filter cake with deionized water 5 times, then place it in a vacuum drying oven, and dry it at 80°C for 3-5h to obtain intermediate B;
[0035] 3: Transfer intermediate B to a distillation tower, control the pressure of the distillation tower to 0.5 atm, and collect the distillation bottom product after distillation for 3-5 hours; transfer the distillation bottom product to room temperature and cool for 1-2 hours to obtain 285 g of modified propylene oxide resin.
[0036] Table 2, reagent parameters used in Example 2
[0037] Drug Name source model parameter Propylene oxide resin Shandong Qiancheng New Materials Co., Ltd. 20220223-1 25kg glacial acetic acid Shandong Baijing New Materials Co., Ltd. 7452 25kg Dextran Xi'an Prius Bioengineering Co., Ltd. 8541 1kg Organic silane coupling agent Zhengzhou Jieyang Chemical Products Co., Ltd. KH-570 5kg
[0038] Example 3
[0039] 1: 100g of resin matrix modified bisphenol A type epoxy resin and 40g of tough filler polyurethane resin were mixed in a reactor, stirred at 65°C and 1200rpm for 30min, then 12g of stearamide was added, stirred at 70°C and 1200rpm for 120min, then vacuum filtered, and the filter cake was washed to obtain a tough resin mixture;
[0040] 2: Add 20g of phthalic acid diester to the tough resin mixture, place the reactor in an air bath, heat to 90°C with steam, heat for 15min, set a magnetic rotor stirrer at the bottom of the reactor, set the speed to 1600rpm and stir for 30min to obtain a hardened tough resin mixture;
[0041] 3: Add 10g aluminum hydroxide, 10g silica powder, 2g p-hydroxybenzoate and 2g phenylene sulfide into the reactor, adjust the temperature of the air bath to 60°C, set the speed of the magnetic rotor stirrer to 600rpm, stir at low speed for 2h to evenly disperse the aluminum hydroxide and silica powder in the mixture matrix, then add 60g E-type glass fiber and 60g C-type glass fiber into the reaction system, transfer the reactor to the oil bath, set the temperature of the oil bath to 160°C, set the speed of the magnetic rotor stirrer to 300rpm and stir for 2h;
[0042] 4: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 1 hour to obtain glass fiber reinforced plastic.
[0043] Table 3, reagent parameters used in Example 3
[0044]
[0045]
[0046] Table 4, Parameters of glass fiber reinforced plastics prepared in Example 3
[0047] Test items Test Standards Test Results Impact resistance / MPa GB / T 21122 684 Heat resistance / ℃ ISO 75-1 218 Flexibility / MPa GB / T 9341 266 Alkali resistance (50% NaOH) GB / T 12087 No abnormality <![CDATA[Acid resistance (10% H2SO4)]]> GB / T 12087 No abnormality Water resistance ISO 175-1 No abnormality Environmental protection level ISO 14000 No abnormality
[0048] Example 4
[0049] 1: 120g of resin matrix modified bisphenol A type epoxy resin and 60g of tough filler polyurethane resin were mixed in a reaction kettle, stirred at 65°C and 1200rpm for 30min, then 12g of imidazole was added, stirred at 70°C and 1200rpm for 120min, then vacuum filtered, and the filter cake was washed to obtain a tough resin mixture;
[0050] 2: Add 30g of tributyl phosphate to the tough resin mixture, place the reactor in an air bath, heat to 90°C with steam, heat for 15min, set a magnetic rotor stirrer at the bottom of the reactor, set the speed to 1600rpm and stir for 30min to obtain a hardened tough resin mixture;
[0051] 3: Add 20g aluminum hydroxide, 20g calcium carbonate, 4g dibenzofuran and 4g dimethylbenzene to the reactor, adjust the temperature of the air bath to 60°C, set the speed of the magnetic rotor stirrer to 800rpm, stir at low speed for 2h to evenly disperse the aluminum hydroxide and calcium carbonate in the mixture matrix, then add 80g E-type glass fiber and 80g C-type glass fiber to the reaction system, transfer the reactor to an oil bath, set the temperature of the oil bath to 180°C, set the speed of the magnetic rotor stirrer to 500rpm and stir for 2h;
[0052] 4: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 1 hour to obtain glass fiber reinforced plastic.
[0053] Table 5, reagent parameters used in Example 3
[0054]
[0055] Table 6, Parameters of glass fiber reinforced plastics prepared in Example 3
[0056] Test items Test Standards Test Results Impact resistance / MPa GB / T 21122 706 Heat resistance / ℃ ISO 75-1 221 Flexibility / MPa GB / T 9341 273 Alkali resistance (50% NaOH) GB / T 12087 No abnormality <![CDATA[Acid resistance (10% H2SO4)]]> GB / T 12087 No abnormality Water resistance ISO 175-1 No abnormality Environmental protection level ISO 14000 No abnormality
[0057] Example 5
[0058] 1: 100g of resin matrix modified propylene oxide resin and 40g of tough filler polyurethane resin were mixed in a reactor, stirred at 65°C and 1200rpm for 30min, then 14g of stearamide was added, stirred at 70°C and 1200rpm for 120min, then vacuum filtered, and the filter cake was washed to obtain a tough resin mixture;
[0059] 2: Add 14g of phthalic acid diester to the tough resin mixture, place the reactor in an air bath, heat to 90°C with steam, heat for 15min, set a magnetic rotor stirrer at the bottom of the reactor, set the speed to 1600rpm and stir for 30min to obtain a hardened tough resin mixture;
[0060] 3: Add 12g of calcium carbonate, 12g of silica powder, 2g of p-hydroxybenzoic acid methyl ester and 2g of phenylene sulfide into the reactor, adjust the temperature of the air bath to 60°C, set the speed of the magnetic rotor stirrer to 600rpm, stir at low speed for 2h to evenly disperse the calcium carbonate and silica powder in the mixture matrix, then add 60g of E-type glass fiber and 60g of C-type glass fiber into the reaction system, transfer the reactor to an oil bath, set the temperature of the oil bath to 160°C, set the speed of the magnetic rotor stirrer to 300rpm and stir for 2h;
[0061] 4: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 1 hour to obtain glass fiber reinforced plastic.
[0062] Table 7, reagent parameters used in Example 3
[0063]
[0064] Table 8, Parameters of glass fiber reinforced plastics prepared in Example 5
[0065]
[0066]
[0067] Comparative Example 1
[0068] 1: Mix 120g of the resin matrix bisphenol A epoxy resin and 60g of the tough filler polyurethane resin in a reactor, stir at 65°C and 1200rpm for 30min, then add 14g of stearamide, stir at 70°C and 1200rpm for 120min, then vacuum filter and wash the filter cake to obtain a tough resin mixture;
[0069] 2: Add 30g of tributyl phosphate to the tough resin mixture, place the reactor in an air bath, heat to 90°C with steam, heat for 15min, set a magnetic rotor stirrer at the bottom of the reactor, set the speed to 1600rpm and stir for 30min to obtain a hardened tough resin mixture;
[0070] 3: Add 20g aluminum hydroxide, 20g calcium carbonate, 4g dibenzofuran and 4g dimethylbenzene to the reactor, adjust the temperature of the air bath to 60°C, set the speed of the magnetic rotor stirrer to 800rpm, stir at a low speed for 2h to evenly disperse the calcium carbonate and aluminum hydroxide in the mixture matrix, then add 80g E-type glass fiber and 80g C-type glass fiber to the reaction system, transfer the reactor to an oil bath, set the temperature of the oil bath to 180°C, set the speed of the magnetic rotor stirrer to 500rpm and stir for 2h;
[0071] 4: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 1 hour to obtain glass fiber reinforced plastic.
[0072] Table 9, parameters of glass fiber reinforced plastics prepared in Comparative Example 1
[0073]
[0074]
[0075] Comparative Example 2
[0076] 1: Mix 100g of resin matrix propylene oxide resin and 40g of tough filler polyurethane resin in a reactor, stir at 65°C and 1200rpm for 30min, then add 12g of imidazole, stir at 70°C and 1200rpm for 120min, then vacuum filter and wash the filter cake to obtain a tough resin mixture;
[0077] 2: Add 30g of phthalic acid diester to the tough resin mixture, place the reactor in an air bath, heat to 90°C with steam, heat for 15min, set a magnetic rotor stirrer at the bottom of the reactor, set the speed to 1600rpm and stir for 30min to obtain a hardened tough resin mixture;
[0078] 3: Add 20g silica powder, 20g calcium carbonate, 4g dibenzofuran and 4g dimethylbenzene to the reactor, adjust the temperature of the air bath to 60°C, set the speed of the magnetic rotor stirrer to 800rpm, stir at low speed for 2h to evenly disperse the calcium carbonate and silica powder in the mixture matrix, then add 80g E-type glass fiber and 80g C-type glass fiber to the reaction system, transfer the reactor to an oil bath, set the temperature of the oil bath to 180°C, set the speed of the magnetic rotor stirrer to 500rpm and stir for 2h;
[0079] 4: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 0.5 h to obtain glass fiber reinforced plastic.
[0080] Table 10, Parameters of glass fiber reinforced plastics prepared in Comparative Example 2
[0081]
[0082]
[0083] Tensile toughness test:
[0084] The glass fiber reinforced plastics prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to performance tests, and the measurement method was determined according to the method described in the American material standard ASTM D4145.
[0085] Table 11, tensile toughness test results of Examples 3-5 and Comparative Examples 1-2
[0086]
[0087] Aging performance test:
[0088] The wet heat aging test was carried out according to the test method of GB / T2423.3. Test conditions: +85℃, relative humidity 85%, 1000h. The tensile strength of the sample was tested before and after the test, and the yellowing index (ΔYI) was measured according to the national standard "Plastic Yellow Index Test Method" GB2409.
[0089] Table 12, aging performance test results of Examples 3-5 and Comparative Examples 1-2
[0090]
[0091]
[0092] Physical properties test
[0093] The glass fiber reinforced plastics prepared in Examples 3-5 and Comparative Examples 1-2 were tested for physical properties.
[0094] Table 13, Physical property test results of Examples 3-5 and Comparative Examples 1-2
[0095] sample Tensile strength / MPa Bending strength / MPa Heat deformation temperature / ℃ Example 3 179 266 215 Example 4 193 273 222 Example 5 175 241 217 Comparative Example 1 171 209 213 Comparative Example 2 168 194 208
[0096] Through the above experimental analysis, it can be known that the glass fiber reinforced plastic prepared by the present invention fully meets the current national standards, and the glass fiber reinforced plastic containing modified epoxy resin has better strength and toughness.
[0097] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A resin-based glass fiber reinforced plastic, characterized in that: The composition comprises the following percentages: modified epoxy resin 25%-30%, polyurethane resin 10%-15%, hardener 5%-15%, glass fiber 30%-50%, initiator 3%-5%, antioxidant 0.5%-3%, light stabilizer 0.5%-3% and filler 5%-10%; The modified epoxy resin is prepared by the following steps: A1: Add epoxy resin and glacial acetic acid into deionized water, heat in an oil bath pot equipped with a thermometer and a magnetic stirrer, stir and react for 30 min at a temperature of 100-120°C and a stirring rate of 500-600 rpm. After complete dissolution, adjust the temperature to 45-60°C, set the stirring rate to 300-400 rpm, and stir for 2 h to obtain intermediate A; A2: Add dextran and organosilane coupling agent to intermediate A, use a flask equipped with a stirrer and a thermometer, tilt the flask mouth at 45 degrees, heat the bottom with an alcohol lamp, stir and react for 30 minutes at a temperature of 30-45°C and a stirring rate of 400-600rpm, then use a serpentine tube and condensed water to reflux the product, and reflux for 5-6 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, wash the filter cake with deionized water for 3-5 times, and then place it in a vacuum drying oven and dry it at a temperature of 80-85°C for 3-5 hours to obtain intermediate B; A3: The intermediate B is transferred to a distillation tower, and the bottom product of the distillation is collected after distillation for 3-5 hours; the bottom product of the distillation is transferred to room temperature and cooled for 1-2 hours to obtain a modified epoxy resin.
2. A resin-based glass fiber reinforced plastic according to claim 1, characterized in that: In step A1, the concentration of glacial acetic acid is 9%; the ratio of glacial acetic acid to deionized water is 1:
10.
3. A resin-based glass fiber reinforced plastic according to claim 1, characterized in that: In step A2, the ratio of intermediate A, dextran and organosilane coupling agent is 10:5:
1.
4. A resin-based glass fiber reinforced plastic according to claim 1, characterized in that: In step A3, the pressure range of the distillation tower is 0.2-0.5 atm.
5. The method for preparing a glass fiber reinforced plastic according to claim 1, characterized in that: The preparation method comprises the following steps: S1: Preparation of modified epoxy resin; S2: Mix the resin matrix modified epoxy resin and the tough filler polyurethane resin in a reaction kettle, stir at 45-65°C and 800-1200rpm for 30min, then add the initiator, stir at 65-70°C and 800-1200rpm for 120min, then vacuum filter and wash the filter cake to obtain a tough resin mixture; S3: adding the hardener to the tough resin mixture, placing the reactor in a gas bath, steam heating to 65-90°C for 15 minutes, setting a magnetic rotor stirrer at the bottom of the reactor, setting the speed to 1000-1600 rpm and stirring for 30 minutes to obtain a hardened tough resin mixture; S4: Add filler, light stabilizer and antioxidant into the reactor, adjust the temperature of the air bath to 55-60°C, set the speed of the magnetic rotor stirrer to 600-800rpm, stir at low speed for 2h to evenly disperse the filler in the mixture matrix, then add glass fiber into the reaction system, transfer the reactor to the oil bath, set the temperature of the oil bath to 160-180°C, set the speed of the magnetic rotor stirrer to 300-500rpm and stir for 2h; S5: After the reaction is completed, the mixture in the reactor is vacuum filtered into a mold and cured for 0.5-1h to obtain a glass fiber reinforced plastic.
6. The resin-based glass fiber reinforced plastic according to claim 1, characterized in that: The epoxy resin is one of bisphenol A epoxy resin, bisphenol F epoxy resin and propylene oxide resin.
7. The resin-based glass fiber reinforced plastic according to claim 1, characterized in that: The glass fibers are E-type glass fibers and C-type glass fibers, and the ratio of the E-type glass fibers to the C-type glass fibers is 1:1.
Citation Information
Cited By
Plugging agent for repairing building roofs and preparation method thereof
CN119177104A
High-strength composite glass and processing technology thereof
CN119661119A