Wear-resistant low-warpage flame-retardant nylon composite material and preparation method thereof
By combining special nylon resin, syngastic polystyrene and other additives, the wear resistance and antistatic problems of nylon composite materials in coin counting machines are solved, and nylon composites with high wear resistance and low warping are achieved. Material preparation ensures the normal operation of the money counting machine and reduces production costs.
Patent Information
- Application Number
- CN202411203583.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In the coin counter, the existing nylon composite materials are insufficient wear resistance, poor anti-static effect and high warping, resulting in surface wear, electrostatic sparks and product deformation, affecting the normal operation of the counter.
Special nylon resin and syngastic polystyrene are used as the main materials, combined with lubricant, wear-resistant masterbatch, carbon nanotubes and flame retardant, and low warpage is prepared through low temperature plasma treatment and twin screw extrusion technology. A nylon composite material with high flatness, excellent wear resistance and chemical resistance enhances its mechanical strength and flame retardant properties.
It realizes the high wear resistance, low warpage, good flame retardant and anti-static effect of nylon composite materials, can withstand 200,000 times of coin counting operations, ensures the normal operation of the cash counter, and simplifies the preparation process and reduces the production costs.
Smart Images

Figure BDA0005018400870000021 
Figure BDA0005018400870000041 
Figure BDA0005018400870000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wear-resistant, low-warping, flame-retardant nylon composite materials, and in particular to a wear-resistant, low-warping, flame-retardant nylon composite material and a preparation method thereof. Background Art
[0002] Nylon engineering plastics are widely used in electronics, automobiles, construction, office equipment, machinery, aerospace and other industries due to their high performance advantages in mechanical properties, durability, corrosion resistance, heat resistance, etc. Replacing steel and wood with plastic has become an international trend.
[0003] A coin counter is a coin sorting machine that can accurately distinguish various coins and display the total amount of coins placed and the number of coins of different denominations. In the use of existing coin counters, due to the high-speed collision and friction between coins and the counter, and the coins usually have residual components such as sweat and oil, it is easy to cause the surface wear of the counter and coin jam during operation. Static electricity / sparks are easily generated between coins and the counter, and between coins. However, the existing nylon composite materials have insufficient wear resistance, poor antistatic and flame retardant effects, and high warping, which causes product deformation, affecting the normal counting operation of the counter. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies in the prior art, one of the objects of the present invention is to provide a wear-resistant, low-warping, flame-retardant nylon composite material with low warping, high flatness, excellent wear resistance and chemical resistance, and better flame retardant and antistatic effects. The composite material is particularly suitable for coin counting machines and can withstand 200,000 coin countings to ensure the normal counting operation of the coin counting machine.
[0005] The second object of the present invention is to provide a method for preparing a wear-resistant, low-warping, flame-retardant nylon composite material, which has simple operation, convenient control, high production efficiency, low production cost, and can be used for large-scale production.
[0006] One of the purposes of the present invention is achieved by the following technical solution: A wear-resistant, low-warping, flame-retardant nylon composite material, comprising the following raw materials in parts by weight:
[0007]
[0008] This wear-resistant, low-warping, flame-retardant nylon composite material has low warping, high flatness, excellent wear resistance and chemical resistance, and better flame retardant and antistatic effects. It is particularly suitable for coin counting machines and can withstand 200,000 coin countings to ensure the normal counting operation of the coin counting machine. Among them, special nylon resin and syndiotactic polystyrene are used as the main materials, which interact with each other to obtain higher rigidity, chemical resistance, dimensional stability, lower water absorption and low warping; the added lubricant can fully lubricate and disperse the wear-resistant masterbatch, wear-resistant filler powder and carbon nanotube masterbatch, and the lubricant, wear-resistant masterbatch and wear-resistant filler powder work synergistically in the special nylon resin to significantly improve the surface hardness and wear resistance of the nylon composite material; the added carbon nanotube masterbatch is evenly dispersed in the nylon composite material, which can not only reduce the resistivity of the nylon composite material to achieve antistatic effect, but also help to enhance the toughness, hardness and wear resistance of nylon, improve its ability to resist external forces, thereby enhancing the overall mechanical strength of the material; the added special flame retardant has high hydrophobicity, hydrolysis resistance and excellent flame retardancy, effectively maintaining its stable fire retardancy and avoiding the migration of flame retardants to the surface during use to affect the overall flame retardancy.
[0009] Preferably, the nylon resin is a PA66 / 6I copolymer, and its relative viscosity is 2.0-2.4; in the PA66 / 6I copolymer, the mass ratio of PA66:PA6I is 6-7:3-4; and the number average molecular weight of the syndiotactic polystyrene is 200,000-1,000,000.
[0010] By adopting the above technical scheme, the mass ratio of PA66:PA6I in the PA66 / 6I copolymer is controlled to be 6-7:3-4, and the excellent performance of PA66 and PA6I (PA6I model: Anaiji A1315) is combined to improve the tensile strength, bending strength and impact strength of the copolymer, especially at high temperatures, it can still maintain good mechanical properties, and is more conducive to obtaining higher rigidity, chemical corrosion resistance, heat resistance, dimensional stability, wear resistance, lower water absorption and low warpage. The number average molecular weight of syndiotactic polystyrene is between 200,000 and 1 million, with good heat resistance, good chemical resistance, and extremely low water absorption, which is conducive to reducing the water absorption of the composite material, maintaining stability, good dimensional stability, and excellent mechanical properties.
[0011] Preferably, the antioxidant is antioxidant 1098 and / or antioxidant S9228.
[0012] The above technical solution is helpful to avoid the degradation of nylon composite materials caused by oxidation during processing and use, thereby improving the heat resistance, durability and stability of nylon composite materials. More preferably, the antioxidant is a mixture of antioxidant 1098 and antioxidant S9228 in a weight ratio of 1:2-3.
[0013] Preferably, the lubricant is at least one of high temperature resistant silicone masterbatch MB50-001, K6105M and HMB-6301.
[0014] The above technical solution is beneficial to increase the lubrication in the system, facilitate demoulding, improve the surface smoothness and feel of the product, reduce the friction coefficient, improve the dispersion and compatibility of wear-resistant masterbatch, wear-resistant filler powder and carbon nanotube masterbatch, and also have good wear resistance and scratch resistance.
[0015] Preferably, the compatibilizer is POE-g-MAH, and its grafting rate is 1.0-1.3MA%.
[0016] The adoption of the above technical solution is beneficial to providing compatibility between materials in the system and at the same time achieving a toughening effect on the nylon composite material.
[0017] Preferably, the particle size of the flame retardant is 10-16 μm, and its chemical structure is as follows:
[0018]
[0019] By adopting the above technical scheme, the flame retardant has a higher phosphorus content, a higher bulk density and glass transition temperature, good dispersion compatibility, high hydrophobicity, hydrolysis resistance and excellent flame retardancy, which effectively maintains its fire retardant performance stable and avoids the migration of the flame retardant to the surface during use and affecting the overall flame retardancy.
[0020] Preferably, the preparation method of the wear-resistant masterbatch comprises the following steps:
[0021] (R1), take 10-20 parts of ultra-high molecular weight polyethylene, 1-3 parts of grafting monomer, 0.01-0.1 parts of initiator, 0.1-0.2 parts of regulator and 100 parts of PA66 with a relative viscosity of 2.4 by weight, and set aside;
[0022] (R2), treating the ultra-high molecular weight polyethylene with nitrogen at low temperature plasma for 5-10 minutes to obtain polarized polyethylene;
[0023] (R3), the polarized polyethylene, grafted monomer, initiator and regulator are mixed uniformly, sent into a screw extruder under nitrogen protection, and extruded and granulated at a temperature of 150-200° C., and then cooled to obtain grafted modified polarized polyethylene;
[0024] (R4) The grafted modified polarized polyethylene and PA66 are evenly dispersed in a high-speed mixer, and extruded into granules through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 190-210°C, 230-250°C, 250-260°C, 250-260°C, 235-245°C, 235-245°C, the head temperature is 230-240°C, and the screw speed is 320-400r / min to obtain wear-resistant masterbatch.
[0025] The above technical solution is used in the preparation process to treat ultra-high molecular weight polyethylene with low-temperature plasma to form new active groups on its surface, increase its reactivity, and then generate modified polyethylene with stronger polarity after grafting reaction with grafting monomers. It has better dispersion compatibility and is more conducive to improving the tear resistance, wear resistance, chemical corrosion resistance and aging resistance of nylon composite materials, and reducing the friction coefficient. Furthermore, the power used for low-temperature plasma treatment is 8kW-15kW and the voltage is 380V.
[0026] Preferably, the number average molecular weight of the ultra-high molecular weight polyethylene is 2 million to 3 million; the grafting monomer is maleic anhydride; the initiator is dicumyl peroxide and / or di-tert-butyl peroxide; and the regulator is zinc dimethyldithiocarbamate.
[0027] By adopting the above technical scheme, the number average molecular weight of ultra-high molecular weight polyethylene is controlled at 2 million to 3 million, and the wear resistance of ultra-high molecular weight polyethylene is enhanced. Its molecular chain is long and highly entangled, so that the material can resist wear during friction and maintain long-term stable performance. In addition, maleic anhydride is used as a grafting monomer, and its polar group can improve the surface wettability of the material, reduce the friction coefficient, thereby improving the lubrication performance, and can form a stronger interaction force with nylon resin and syndiotactic polystyrene, thereby improving the interface bonding force between it and the substrate, dispersing more evenly, and avoiding shedding or stratification during use. It helps to control the rate and degree of grafting reaction and avoid the degradation of material performance caused by excessive grafting. The regulator uses zinc dimethyldithiocarbamate, which helps to control the rate and degree of grafting reaction, avoid the degradation of material performance caused by excessive grafting, and at the same time, improve the processing fluidity of wear-resistant masterbatch.
[0028] Preferably, the wear-resistant filling powder is nano-aluminum oxide and / or nano-silicon carbide; the carbon nanotube masterbatch is made by melt-granulating PA66 with a relative viscosity of 2.4 as a carrier and carbon nanotubes, the carbon nanotube content is 14-18wt%, the carbon nanotube diameter is 8-12nm, and the carbon nanotube length is 30-50μm.
[0029] By adopting the above technical scheme, the nano silicon carbide powder has good compatibility and dispersibility in nylon resin, is closely combined with the matrix, improves the surface hardness of nylon composite materials, increases elastic modulus, significantly improves the tensile strength and wear resistance of nylon composite materials, plays a lubricating and filling role, and can reduce friction and wear between materials; more preferably, the wear-resistant filling powder is a mixture of nano aluminum oxide and nano silicon carbide in a weight ratio of 1:5-8, and the nano aluminum oxide is obtained by immersing nano aluminum oxide in KH-560 coupling agent for 10-20 hours and filtering out the coupling agent, and the KH-560 coupling agent is adsorbed on the surface of nano aluminum oxide, reducing the interaction between particles, avoiding the agglomeration of nano aluminum oxide, and helping the uniform dispersion of nano aluminum oxide in nylon composite materials. The added carbon nanotube masterbatch is evenly dispersed in the nylon composite material, which can not only reduce the resistivity of the nylon composite material and achieve antistatic effect, but also help to enhance the toughness, hardness and wear resistance of nylon, improve its ability to resist external forces, and thus enhance the overall mechanical strength of the material.
[0030] The second object of the present invention is achieved by the following technical solution: The preparation method of the above-mentioned wear-resistant, low-warping, flame-retardant nylon composite material comprises the following steps:
[0031] (S1), taking nylon resin, syndiotactic polystyrene, antioxidant, lubricant, compatibilizer, flame retardant, wear-resistant masterbatch, wear-resistant filling powder and carbon nanotube masterbatch according to weight parts, and setting aside;
[0032] (S2), premixing nylon resin with 0.1 parts of diffusion oil in a high-speed mixer for 2 minutes, and then blending with other raw materials for 2 minutes before discharging, and extruding and granulating through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, the head temperature is 270-290°C, and the screw speed is 500r / min to obtain a wear-resistant, low-warpage, flame-retardant nylon composite material.
[0033] The beneficial effects of the present invention are as follows: the wear-resistant, low-warping, flame-retardant nylon composite material of the present invention has low warping, high flatness, excellent wear resistance and chemical resistance, and better flame retardant and antistatic effects, and is particularly suitable for coin counting machines, and can withstand 200,000 coin countings, thereby ensuring the normal counting operation of the coin counting machine. Among them, special nylon resin and syndiotactic polystyrene are used as the main materials, which interact with each other to obtain higher rigidity, chemical resistance, dimensional stability, lower water absorption and low warping; the added lubricant can fully lubricate and disperse the wear-resistant masterbatch, wear-resistant filler powder and carbon nanotube masterbatch, and the lubricant, wear-resistant masterbatch and wear-resistant filler powder work synergistically in the special nylon resin to significantly improve the surface hardness and wear resistance of the nylon composite material; the added carbon nanotube masterbatch is evenly dispersed in the nylon composite material, which can not only reduce the resistivity of the nylon composite material to achieve antistatic effect, but also help to enhance the toughness, hardness and wear resistance of nylon, improve its ability to resist external forces, thereby enhancing the overall mechanical strength of the material; the added special flame retardant has high hydrophobicity, hydrolysis resistance and excellent flame retardancy, effectively maintaining its stable fire retardancy and avoiding the migration of flame retardants to the surface during use to affect the overall flame retardancy.
[0034] The preparation method of the invention has the advantages of simple operation, convenient control, high production efficiency and low production cost, and can be used for large-scale production. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0036] Example 1
[0037] A wear-resistant, low-warping, flame-retardant nylon composite material, comprising the following raw materials in parts by weight:
[0038]
[0039] The nylon resin is a PA66 / 6I copolymer, and its relative viscosity is 2.0; in the PA66 / 6I copolymer, the mass ratio of PA66:PA6I is 7:3; the number average molecular weight of the syndiotactic polystyrene is 500,000.
[0040] The antioxidant is a mixture of antioxidant 1098 and antioxidant S9228 in a weight ratio of 1:2.8.
[0041] The lubricant is high temperature resistant silicone masterbatch MB50-001.
[0042] The compatibilizer is POE-g-MAH, and its grafting rate is 1.2MA%.
[0043] The particle size of the flame retardant is 13 μm, and its chemical structure is as follows:
[0044]
[0045] The preparation method of the wear-resistant masterbatch comprises the following steps:
[0046] (R1), take 15 parts of ultra-high molecular weight polyethylene, 2 parts of grafting monomer, 0.05 parts of initiator, 0.15 parts of regulator and 100 parts of PA66 with a relative viscosity of 2.4 by weight, and set aside;
[0047] (R2), treating the ultra-high molecular weight polyethylene with nitrogen at low temperature plasma for 6 min to obtain polarized polyethylene;
[0048] (R3), the polarized polyethylene, grafted monomer, initiator and regulator are mixed uniformly, sent into a screw extruder under nitrogen protection, and extruded and granulated at 180° C., and then cooled to obtain grafted modified polarized polyethylene;
[0049] (R4) The grafted modified polarized polyethylene and PA66 are evenly dispersed in a high-speed mixer, and granulated by extrusion through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 240°C, 255°C, 255°C, 240°C, 240°C, the head temperature is 235°C, and the screw speed is 380r / min to obtain wear-resistant masterbatch.
[0050] The number average molecular weight of the ultra-high molecular weight polyethylene is 2.5 million; the grafting monomer is maleic anhydride; the initiator is dicumyl peroxide; the regulator is zinc dimethyldithiocarbamate. The power used for low temperature plasma treatment is 10 kW and the voltage is 380V.
[0051] The wear-resistant filling powder is a mixture of nano-aluminum oxide and nano-silicon carbide in a weight ratio of 1:7, and the nano-aluminum oxide is prepared by immersing the nano-aluminum oxide in a KH-560 coupling agent for 12 hours and then filtering out the coupling agent; the carbon nanotube masterbatch is prepared by using PA66 with a relative viscosity of 2.4 as a carrier and melt-granulating with carbon nanotubes, the content of the carbon nanotubes is 15wt%, the diameter of the carbon nanotubes is 10nm, and the length of the carbon nanotubes is 40μm.
[0052] The preparation method of the wear-resistant, low-warping, flame-retardant nylon composite material comprises the following steps:
[0053] (S1), taking nylon resin, syndiotactic polystyrene, antioxidant, lubricant, compatibilizer, flame retardant, wear-resistant masterbatch, wear-resistant filling powder and carbon nanotube masterbatch according to weight parts, and setting aside;
[0054] (S2) Premix the nylon resin with 0.1 parts of diffusion oil in a high-speed mixer for 2 minutes, then blend with other raw materials for 2 minutes and discharge the mixture, and extrude and granulate it through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 260°C, 270°C, 280°C, 270°C, 260°C, 260°C, 260°C, 260°C, 260°C, and 260°C, respectively. The head temperature is 270°C and the screw speed is 500r / min to obtain a wear-resistant, low-warpage, flame-retardant nylon composite material.
[0055] Example 2
[0056] A wear-resistant, low-warping, flame-retardant nylon composite material, comprising the following raw materials in parts by weight:
[0057]
[0058] The nylon resin is a PA66 / 6I copolymer, and its relative viscosity is 2.0; in the PA66 / 6I copolymer, the mass ratio of PA66:PA6I is 7:3; the number average molecular weight of the syndiotactic polystyrene is 500,000.
[0059] The antioxidant is a mixture of antioxidant 1098 and antioxidant S9228 in a weight ratio of 1:2.
[0060] The lubricant is high temperature resistant silicone masterbatch MB50-001.
[0061] The compatibilizer is POE-g-MAH, and its grafting rate is 1.2MA%.
[0062] The particle size of the flame retardant is 16 μm, and its chemical structure is as follows:
[0063]
[0064] The preparation method of the wear-resistant masterbatch comprises the following steps:
[0065] (R1), take 10 parts of ultra-high molecular weight polyethylene, 1 part of grafting monomer, 0.01 parts of initiator, 0.1 parts of regulator and 100 parts of PA66 with a relative viscosity of 2.4 by weight, and set aside;
[0066] (R2), treating the ultra-high molecular weight polyethylene with nitrogen at low temperature plasma for 5 min to obtain polarized polyethylene;
[0067] (R3), the polarized polyethylene, grafted monomer, initiator and regulator are mixed uniformly, sent into a screw extruder under nitrogen protection, and extruded and granulated at 180° C., and then cooled to obtain grafted modified polarized polyethylene;
[0068] (R4) The grafted modified polarized polyethylene and PA66 are evenly dispersed in a high-speed mixer, and granulated by extrusion through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 190°C, 230°C, 250°C, 250°C, 235°C, 235°C, the head temperature is 230°C, and the screw speed is 380r / min to obtain wear-resistant masterbatch.
[0069] The number average molecular weight of the ultra-high molecular weight polyethylene is 2 million; the grafting monomer is maleic anhydride; the initiator is dicumyl peroxide; the regulator is zinc dimethyldithiocarbamate. The power used for low temperature plasma treatment is 10 kW and the voltage is 380V.
[0070] The wear-resistant filling powder is a mixture of nano-aluminum oxide and nano-silicon carbide in a weight ratio of 1:5, and the nano-aluminum oxide is prepared by immersing the nano-aluminum oxide in a KH-560 coupling agent for 12 hours and then filtering out the coupling agent; the carbon nanotube masterbatch is prepared by using PA66 with a relative viscosity of 2.4 as a carrier and melt-granulating with carbon nanotubes, the content of the carbon nanotubes is 14wt%, the diameter of the carbon nanotubes is 12nm, and the length of the carbon nanotubes is 50μm.
[0071] The preparation method of the wear-resistant, low-warping, flame-retardant nylon composite material comprises the following steps:
[0072] (S1), taking nylon resin, syndiotactic polystyrene, antioxidant, lubricant, compatibilizer, flame retardant, wear-resistant masterbatch, wear-resistant filling powder and carbon nanotube masterbatch according to weight parts, and setting aside;
[0073] (S2) Premix the nylon resin with 0.1 parts of diffusion oil in a high-speed mixer for 2 minutes, then blend with other raw materials for 2 minutes and discharge the mixture, and extrude and granulate it through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 260°C, 270°C, 280°C, 270°C, 260°C, 260°C, 260°C, 260°C, 260°C, and 260°C, respectively. The head temperature is 270°C and the screw speed is 500r / min to obtain a wear-resistant, low-warpage, flame-retardant nylon composite material.
[0074] Example 3
[0075] A wear-resistant, low-warping, flame-retardant nylon composite material, comprising the following raw materials in parts by weight:
[0076]
[0077] The nylon resin is a PA66 / 6I copolymer, and its relative viscosity is 2.0; in the PA66 / 6I copolymer, the mass ratio of PA66:PA6I is 7:3; the number average molecular weight of the syndiotactic polystyrene is 500,000.
[0078] The antioxidant is a mixture of antioxidant 1098 and antioxidant S9228 in a weight ratio of 1:3.
[0079] The lubricant is high temperature resistant silicone masterbatch MB50-001.
[0080] The compatibilizer is POE-g-MAH, and its grafting rate is 1.2MA%.
[0081] The particle size of the flame retardant is 10 μm, and its chemical structure is as follows:
[0082]
[0083] The preparation method of the wear-resistant masterbatch comprises the following steps:
[0084] (R1), take 20 parts of ultra-high molecular weight polyethylene, 3 parts of grafting monomer, 0.1 parts of initiator, 0.2 parts of regulator and 100 parts of PA66 with a relative viscosity of 2.4 by weight, and set aside;
[0085] (R2), treating the ultra-high molecular weight polyethylene with nitrogen at low temperature plasma for 10 min to obtain polarized polyethylene;
[0086] (R3), the polarized polyethylene, grafted monomer, initiator and regulator are mixed uniformly, sent into a screw extruder under nitrogen protection, and extruded and granulated at 180° C., and then cooled to obtain grafted modified polarized polyethylene;
[0087] (R4) The grafted modified polarized polyethylene and PA66 are evenly dispersed in a high-speed mixer, and extruded into granules through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 210°C, 250°C, 260°C, 260°C, 245°C, 245°C, the head temperature is 240°C, and the screw speed is 380r / min to obtain wear-resistant masterbatch.
[0088] The number average molecular weight of the ultra-high molecular weight polyethylene is 3 million; the grafting monomer is maleic anhydride; the initiator is dicumyl peroxide; the regulator is zinc dimethyldithiocarbamate. The power used for low temperature plasma treatment is 10 kW and the voltage is 380V.
[0089] The wear-resistant filling powder is a mixture of nano-aluminum oxide and nano-silicon carbide in a weight ratio of 1:8, and the nano-aluminum oxide is prepared by immersing the nano-aluminum oxide in a KH-560 coupling agent for 12 hours and then filtering out the coupling agent; the carbon nanotube masterbatch is prepared by using PA66 with a relative viscosity of 2.4 as a carrier and melt-granulating with carbon nanotubes, the content of the carbon nanotubes is 18wt%, the diameter of the carbon nanotubes is 8nm, and the length of the carbon nanotubes is 30μm.
[0090] The preparation method of the wear-resistant, low-warping, flame-retardant nylon composite material comprises the following steps:
[0091] (S1), taking nylon resin, syndiotactic polystyrene, antioxidant, lubricant, compatibilizer, flame retardant, wear-resistant masterbatch, wear-resistant filling powder and carbon nanotube masterbatch according to weight parts, and setting aside;
[0092] (S2) Premix the nylon resin with 0.1 parts of diffusion oil in a high-speed mixer for 2 minutes, then blend with other raw materials for 2 minutes and discharge the mixture, and extrude and granulate it through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 260°C, 270°C, 280°C, 270°C, 260°C, 260°C, 260°C, 260°C, 260°C, and 260°C, respectively. The head temperature is 270°C and the screw speed is 500r / min to obtain a wear-resistant, low-warpage, flame-retardant nylon composite material.
[0093] Example 4
[0094] A wear-resistant, low-warping, flame-retardant nylon composite material, comprising the following raw materials in parts by weight:
[0095]
[0096]
[0097] The nylon resin is a PA66 / 6I copolymer, and its relative viscosity is 2.0; in the PA66 / 6I copolymer, the mass ratio of PA66:PA6I is 7:3; the number average molecular weight of the syndiotactic polystyrene is 500,000.
[0098] The antioxidant is a mixture of antioxidant 1098 and antioxidant S9228 in a weight ratio of 1:2.3.
[0099] The lubricant is high temperature resistant silicone masterbatch MB50-001.
[0100] The compatibilizer is POE-g-MAH, and its grafting rate is 1.2MA%.
[0101] The particle size of the flame retardant is 13 μm, and its chemical structure is as follows:
[0102]
[0103] The preparation method of the wear-resistant masterbatch comprises the following steps:
[0104] (R1), take 16 parts of ultra-high molecular weight polyethylene, 1.6 parts of grafting monomer, 0.06 parts of initiator, 0.16 parts of regulator and 100 parts of PA66 with a relative viscosity of 2.4 by weight, and set aside;
[0105] (R2), treating the ultra-high molecular weight polyethylene with nitrogen at low temperature plasma for 6 min to obtain polarized polyethylene;
[0106] (R3), the polarized polyethylene, grafted monomer, initiator and regulator are mixed uniformly, sent into a screw extruder under nitrogen protection, and extruded and granulated at 180° C., and then cooled to obtain grafted modified polarized polyethylene;
[0107] (R4) The grafted modified polarized polyethylene and PA66 are evenly dispersed in a high-speed mixer, and granulated by extrusion through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 240°C, 255°C, 255°C, 240°C, 240°C, the head temperature is 235°C, and the screw speed is 380r / min to obtain wear-resistant masterbatch.
[0108] The number average molecular weight of the ultra-high molecular weight polyethylene is 2.8 million; the grafting monomer is maleic anhydride; the initiator is dicumyl peroxide; the regulator is zinc dimethyldithiocarbamate. The power used for low temperature plasma treatment is 10 kW and the voltage is 380V.
[0109] The wear-resistant filling powder is a mixture of nano-aluminum oxide and nano-silicon carbide in a weight ratio of 1:7, and the nano-aluminum oxide is prepared by immersing the nano-aluminum oxide in a KH-560 coupling agent for 12 hours and then filtering out the coupling agent; the carbon nanotube masterbatch is prepared by using PA66 with a relative viscosity of 2.4 as a carrier and melt-granulating with carbon nanotubes, the content of the carbon nanotubes is 16wt%, the diameter of the carbon nanotubes is 10nm, and the length of the carbon nanotubes is 38μm.
[0110] The preparation method of the wear-resistant, low-warping, flame-retardant nylon composite material comprises the following steps:
[0111] (S1), taking nylon resin, syndiotactic polystyrene, antioxidant, lubricant, compatibilizer, flame retardant, wear-resistant masterbatch, wear-resistant filling powder and carbon nanotube masterbatch according to weight parts, and setting aside;
[0112] (S2) Premix the nylon resin with 0.1 parts of diffusion oil in a high-speed mixer for 2 minutes, then blend with other raw materials for 2 minutes and discharge the mixture, and extrude and granulate it through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 260°C, 270°C, 280°C, 270°C, 260°C, 260°C, 260°C, 260°C, 260°C, and 260°C, respectively. The head temperature is 270°C and the screw speed is 500r / min to obtain a wear-resistant, low-warpage, flame-retardant nylon composite material.
[0113] Comparative Example 1
[0114] The difference between this comparative example and Example 1 is:
[0115] The nylon resin is a mixture of PA66 (relative viscosity of 2.4) and PA6I (model: Anaiji A1315) in a weight ratio of 7:3.
[0116] Comparative Example 2
[0117] The difference between this comparative example and Example 1 is:
[0118] The flame retardant is aluminum diethylphosphinate FR-13.
[0119] Comparative Example 3
[0120] The difference between this comparative example and Example 1 is:
[0121] The preparation method of the wear-resistant masterbatch comprises the following steps:
[0122] (R1), take 17 parts by weight of ultra-high molecular weight polyethylene with a number average molecular weight of 2.5 million and 100 parts of PA66 with a relative viscosity of 2.4, and set aside;
[0123] (R2) Disperse the ultra-high molecular weight polyethylene and PA66 evenly in a high-speed mixer, and extrude and granulate them through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 240°C, 255°C, 255°C, 240°C, 240°C, the head temperature is 235°C, and the screw speed is 380r / min to obtain wear-resistant masterbatch.
[0124] Performance Testing
[0125] The nylon composite materials of Examples 1-4 and Comparative Examples 1-3 were tested for impact strength, tensile strength, flexural strength, dimensional shrinkage, flame retardant index, surface resistivity, wear loss and wear resistance coefficient. The test results are shown in Table 1 below:
[0126]
[0127]
[0128] It can be seen from Table 1 above that the wear-resistant, low-warpage, flame-retardant nylon composite material of the present invention has a lower shrinkage rate, is beneficial to reducing warpage, improving flatness and dimensional stability, has better wear resistance, and has good flame retardant and antistatic effects.
[0129] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A wear-resistant, low-warping, flame-retardant nylon composite material, characterized in that: The invention comprises the following raw materials in parts by weight:
2. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The nylon resin is a PA66 / 6I copolymer, and its relative viscosity is 2.0-2.4; in the PA66 / 6I copolymer, the mass ratio of PA66:PA6I is 6-7:3-4; the number average molecular weight of the syndiotactic polystyrene is 200,000-1,000,000.
3. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The antioxidant is antioxidant 1098 and / or antioxidant S9228.
4. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The lubricant is at least one of high temperature resistant silicone masterbatch MB50-001, K6105M and HMB-6301.
5. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The compatibilizer is POE-g-MAH, and its grafting rate is 1.0-1.3MA%.
6. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The particle size of the flame retardant is 10-16 μm, and its chemical structure is as follows:
7. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The preparation method of the wear-resistant masterbatch comprises the following steps: (R1), take 10-20 parts of ultra-high molecular weight polyethylene, 1-3 parts of grafting monomer, 0.01-0.1 parts of initiator, 0.1-0.2 parts of regulator and 100 parts of PA66 with a relative viscosity of 2.4 by weight, and set aside; (R2), treating the ultra-high molecular weight polyethylene with nitrogen at low temperature plasma for 5-10 minutes to obtain polarized polyethylene; (R3), the polarized polyethylene, grafted monomer, initiator and regulator are mixed uniformly, sent into a screw extruder under nitrogen protection, and extruded and granulated at a temperature of 150-200° C., and then cooled to obtain grafted modified polarized polyethylene; (R4) The grafted modified polarized polyethylene and PA66 are evenly dispersed in a high-speed mixer, and extruded into granules through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 190-210°C, 230-250°C, 250-260°C, 250-260°C, 235-245°C, 235-245°C, the head temperature is 230-240°C, and the screw speed is 320-400r / min to obtain wear-resistant masterbatch.
8. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 7, characterized in that: The number average molecular weight of the ultra-high molecular weight polyethylene is 2 million to 3 million; the grafting monomer is maleic anhydride; the initiator is dicumyl peroxide and / or di-tert-butyl peroxide; and the regulator is zinc dimethyldithiocarbamate.
9. The wear-resistant, low-warping, flame-retardant nylon composite material according to claim 1, characterized in that: The wear-resistant filling powder is nano-aluminum oxide and / or nano-silicon carbide; the carbon nanotube masterbatch is made by melt-granulating carbon nanotubes with PA66 having a relative viscosity of 2.4 as a carrier, the carbon nanotube content is 14-18wt%, the diameter of the carbon nanotube is 8-12nm, and the length of the carbon nanotube is 30-50μm.
10. A method for preparing the wear-resistant, low-warping, flame-retardant nylon composite material according to any one of claims 1 to 9, characterized in that: The steps include: (S1), taking nylon resin, syndiotactic polystyrene, antioxidant, lubricant, compatibilizer, flame retardant, wear-resistant masterbatch, wear-resistant filling powder and carbon nanotube masterbatch according to weight parts, and setting aside; (S2), premixing nylon resin with 0.1 parts of diffusion oil in a high-speed mixer for 2 minutes, blending with other raw materials for 2 minutes and then discharging the mixture, and extruding and granulating the mixture through a twin-screw extruder. The processing temperatures of each section of the twin-screw extruder starting from the feeding section are: 200°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, 260-280°C, the head temperature is 270-290°C, and the screw speed is 500r / min to obtain a wear-resistant, low-warpage, flame-retardant nylon composite material.
Citation Information
Cited By